Composite film layer, preparation method thereof and bathroom product
By forming a composite film layer of the transition metal layer and the AlFeCrNiCo high-entropy alloy oxide layer in an inert gas vacuum environment, the problems of narrow interference thickness range and complex process of the preparation of blue decorative layer in the prior art are solved, and stability and environmental protection are achieved The preparation of blue film layer improves the overall performance of the film layer.
Patent Information
- Application Number
- CN202411183877.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The prior art has a narrow interference thickness window when preparing the blue decorative layer, difficult operation and complex process, and has a great impact on the environment, making it difficult to achieve mass production.
The transition metal layer is formed by ion coating in an inert gas vacuum environment, and then the AlFeCrNiCo high-entropy alloy layer and its oxide layer are formed by sputtering coating in the same environment to form a closely connected composite film layer, using a variety of physics Vapor phase deposition technology reduces the use of organic coatings and reduces VOC gas emissions.
It realizes the preparation of a stable and environmentally friendly blue composite film layer, which improves the comprehensive performance of the film layer, such as high strength, wear resistance, scratch resistance and high temperature oxidation resistance, and solves the problems of narrow interference thickness range and complex process. Suitable for mass production.
Smart Images

Figure CN119061354A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to, but is not limited to, the field of materials, and in particular to a composite film layer and a preparation method thereof, and sanitary ware. Background Art
[0002] The physical vapor deposition (PVD) coatings of existing kitchen and bathroom hardware products on the market, such as faucets and showers, generally use metal targets such as zirconium and titanium to react with nitrogen, acetylene or methane to deposit decorative films in various colors such as gold, rose gold, and imitation stainless steel color.
[0003] However, the current technology for obtaining a blue decorative layer has many shortcomings. For example, when preparing a blue coating using TiO2, the thickness range of the coating is usually controlled, and the light transmittance and interference phenomenon of light are used to present a blue hue within a specific range of coating thickness. However, this type of technology has the disadvantages of being prone to a narrow interference thickness range window and being difficult to operate and achieve mass production. In addition, the existing blue coating is mostly prepared by spraying high entropy alloy powder onto the substrate, which has a complex process, poor coating adhesion, and a greater impact on the environment.
[0004] Therefore, there is a need for a composite film layer for displaying blue, a preparation method thereof, and a sanitary ware that at least overcomes the above-mentioned problems. Summary of the invention
[0005] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.
[0006] In one aspect, the present application provides a composite film layer, comprising:
[0007] Base material;
[0008] A transition metal layer is formed on the substrate by an ion plating method based on a first target in a vacuum environment containing an inert gas;
[0009] An AlFeCrNiCo high entropy alloy layer, which is located on the transition metal layer and is formed by a sputtering coating method based on a second target in a vacuum environment containing an inert gas; and
[0010] An AlFeCrNiCo high entropy alloy oxide layer, which is located on the AlFeCrNiCo high entropy alloy layer and is formed by a sputtering coating method based on the second target in a vacuum environment containing an inert gas and oxygen;
[0011] wherein the first target material is formed of one or more of metals Zr, Ti and Cr;
[0012] The second target is formed by powder metallurgy using metal powders of Al, Fe, Cr, Ni and Co in an atomic percentage of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1.
[0013] In one embodiment, the second target is formed of metal powders of Al, Fe, Cr, Ni and Co with an atomic percentage of 1:1:1:1:1 via powder metallurgy.
[0014] In one embodiment, the thickness of the transition metal layer is in the range of 10nm to 50nm, the thickness of the AlFeCrNiCo high entropy alloy layer is in the range of 50nm to 100nm, and the thickness of the AlFeCrNiCo high entropy alloy oxide layer is in the range of 50nm to 100nm.
[0015] In one embodiment, the LAB values of the AlFeCrNiCo high entropy alloy oxide layer are L = 23 ± 4, a = -3 ± 1 and b = -24 ± 2. Therefore, in the present application, the composite film layer may also be referred to as a blue composite film layer.
[0016] In another aspect, the present application provides a method for preparing a composite film layer, the method comprising the following steps:
[0017] 1) placing a pretreated substrate, at least one first target material, and at least one second target material in a coating machine;
[0018] 2) evacuating the coating machine and continuously introducing an inert gas, turning on a first power source corresponding to the first target material, and forming a metal transition layer on the substrate by an ion plating method;
[0019] 3) turning off the first power supply and turning on a second power supply corresponding to the second target material, and forming an AlFeCrNiCo high entropy alloy layer on the metal transition layer by a sputtering coating method; and
[0020] 4) continuously introducing oxygen into the coating machine, and forming an AlFeCrNiCo high entropy alloy oxide layer on the AlFeCrNiCo high entropy alloy layer by a sputtering coating method, thereby obtaining the composite film layer;
[0021] The first target material is formed of one or more of metals Zr, Ti, and Cr;
[0022] The second target is formed by powder metallurgy using metal powders of Al, Fe, Cr, Ni and Co in an atomic percentage of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1.
[0023] In one embodiment, step 2) may further include setting the vacuum degree at 8×10 -4 ~6×10 -3 Pa, the flow rate of the inert gas is set in the range of 20 to 60 sccm, and the pressure in the coating machine is maintained at 8×10 -2 ~7×10 -1 Within the range of Pa.
[0024] In one embodiment, step 4) further comprises applying a bias voltage of -100 to -200 V to the substrate, the metal transition layer, and the AlFeCrNiCo high entropy alloy layer, and maintaining the pressure in the coating machine at 8×10 -2 ~7×10 -1 Pa range, the coating temperature is set at 100℃~200℃, the coating time is set at 600~1800s, the voltage is set at 350~600V, the current is set at 2~5A, and the argon flow rate is 20~60sccm and the oxygen flow rate is 20~60sccm.
[0025] In other embodiments, step 2) may further include applying a bias voltage of -100 to -300 V to the substrate, setting the coating temperature at 100 to 150° C., setting the coating time at 60 to 120 s, setting the voltage at 20 to 40 V, and setting the current at 50 to 150 A.
[0026] In other embodiments, step 3) may further include setting the coating temperature within the range of 100 to 150° C. and the coating time within the range of 600 to 1800 s.
[0027] In other embodiments, step 3) may further include applying a bias voltage of -50 to -150 V to the substrate and the metal transition layer, the voltage is set in the range of 350 to 600 V, and the current is set in the range of 2 to 5 A.
[0028] In another aspect, the present application provides a bathroom product having a composite film layer, wherein the composite film layer is the composite film layer described above or is produced by the method described above.
[0029] In the present application, the term "bathroom products" may refer to products whose surface is coated or decorated with the blue composite film layer of the present application by other means, including but not limited to faucets, showers, bath cabinets, shower heads, shower heads, spray guns, and floor drains.
[0030] The present application adopts a variety of physical vapor deposition techniques to prepare a composite film layer including a metal transition layer, an AlFeCrNiCo high entropy alloy layer and an AlFeCrNiCo high entropy alloy oxide layer that are closely connected between the layers on the substrate, and the composite film layer can show a blue color. The present application reduces the use of organic coatings and reduces the emission of VOC gases by adopting physical vapor deposition technology, thereby achieving the purpose of environmental protection and pollution-free.
[0031] The present application solves the shortcomings of narrow interference thickness range window and difficulty in mass production when conventional PVD TiO2 is used to prepare blue coating, and avoids color changes of optical films caused by uneven coating.
[0032] The AlFeCrNiCo high entropy alloy layer and AlFeCrNiCo high entropy alloy oxide layer in the composite film layer of the present application have excellent properties such as high strength / hardness, high toughness, high wear resistance, scratch resistance, high corrosion resistance, and high-temperature oxidation resistance, which improves the comprehensive performance of the composite film layer.
[0033] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be invented and obtained by the schemes described in the description. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The accompanying drawings are used to provide an understanding of the technical solution of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present application and do not constitute a limitation on the technical solution of the present application.
[0035] Figure 1 A schematic cross-sectional view of a composite film layer provided for an exemplary embodiment of the present disclosure;
[0036] Figure 2 A photograph of the appearance of the composite film layer provided in Example 1 of the present disclosure; and
[0037] Figure 3 This is a SEM photograph of the composite membrane layer provided in Example 1 of the present disclosure. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application are described in detail below. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.
[0039] refer to Figure 1The present application provides a composite film layer, including a substrate 10, a transition metal layer 20 located on the substrate 10, a wear-resistant and hard AlFeCrNiCo high entropy alloy layer 30 located on the transition metal layer 20, and an AlFeCrNiCo high entropy alloy oxide layer 40 located on the AlFeCrNiCo high entropy alloy layer 30.
[0040] In the present application, the transition metal layer 20 may be formed by an ion plating method using a first target in a vacuum environment containing an inert gas.
[0041] Ion plating can be performed by multi-arc ion plating and other methods. Multi-arc ion plating uses arc discharge to directly generate plasma, has a high ionization rate, deposition rate and good bonding force, and is suitable for forming a transition layer between the substrate and other film layers in this application.
[0042] The AlFeCrNiCo high entropy alloy layer 30 may be formed by a sputtering method using a second target in a vacuum environment containing an inert gas.
[0043] The AlFeCrNiCo high entropy alloy oxide layer 40 may be formed by a sputtering method using a second target in a vacuum environment containing an inert gas and oxygen.
[0044] Sputtering coating can adopt planar target sputtering method.
[0045] In the present application, the substrate suitable for the present application may include but is not limited to stainless steel, aluminum alloy, zinc alloy, copper alloy, electroplatable plastics with electroplated copper, nickel, and chromium coatings.
[0046] In the present application, the first target material may be formed of one or more of metals Zr, Ti, and Cr. The second target material may be formed of metal powders of Al, Fe, Cr, Ni, and Co in an atomic percentage of 0.9 to 1.1:0.9 to 1.1:0.9 to 1.1:0.9 to 1.1:0.9 to 1.1. In other embodiments, the second target material is formed of metal powders of Al, Fe, Cr, Ni, and Co in an atomic percentage of 1:1:1:1:1.
[0047] In the present application, the second target material may be formed by powder metallurgy.
[0048] In the present application, the pretreatment may adopt conventional pretreatment methods in the art, such as grinding and polishing, degreasing with acetone and anhydrous ethanol, ultrasonic cleaning, acid solution cleaning, alkaline solution neutralization, deionized water rinsing, preservative rinsing, etc.
[0049] The present application also provides a method for preparing a composite film layer, comprising the following steps: 1) placing a pretreated substrate, at least one first target material, and at least one second target material in a coating machine; 2) evacuating the coating machine and continuously introducing an inert gas, turning on a first power supply corresponding to the first target material, and using an ion plating method to generate a metal transition layer on the substrate; 3) turning off the first power supply and turning on a second power supply corresponding to the second target material, and using a sputtering coating method to generate an AlFeCrNiCo high entropy alloy layer on the metal transition layer; and 4) continuously introducing oxygen into the coating machine, and using a sputtering coating method to generate an AlFeCrNiCo high entropy alloy oxide layer on the high entropy alloy layer, thereby obtaining a composite film layer.
[0050] In the present application, the number of targets that can be set varies according to the size of the coating machine. For example, in the present application, a column of two first targets and a column of one second target can be set in the coating machine.
[0051] The following examples specifically describe the method for preparing the composite membrane layer of the present application.
[0052] Example 1
[0053] 1. A first target material is formed of Zr metal; Al, Fe, Cr, Ni and Co metal powders are uniformly mixed in a ratio of 1:1:1:1:1 in atomic percentage, and an alloy with a specific shape prepared by a powder metallurgy method is used as a second target material.
[0054] 2. Pretreatment of substrate: The substrate is made of 304 stainless steel; the surface of the substrate is ground and polished, then ultrasonically cleaned with acetone, deionized water and alcohol and then dried.
[0055] 3. Install a substrate, a first target material and a second target material in a vacuum coating machine, wherein the first target material for multi-arc ion coating includes a row of two zirconium targets, and the second target material for sputtering coating includes a row of one high entropy alloy target.
[0056] 4. Preparation of metal transition layer: Use Zr target as base, pre-evacuate to a vacuum degree of 6×10 -3 Pa, the argon gas flow rate was 25 sccm, and the pressure in the coating machine was maintained at 3.5×10 -1 Pa; turn on the multi-arc ion plating power supply, the voltage is 21V, the current is 70A, and the plating time is 120s; during plating, the negative bias voltage is -200V, and the plating temperature is 130℃.
[0057] 5. Preparation of AlFeCrNiCo high entropy alloy layer: turn off the multi-arc ion plating power supply for preparing the metal transition layer in step 4, turn on the planar target sputtering coating power supply, the voltage is 450V, the current is 2.5A, and the coating time is 1200s; the negative bias voltage during coating is -100V, and the coating temperature is 130°C.
[0058] 6. Preparation of AlFeCrNiCo high entropy alloy oxide layer: simultaneously inject argon flow rate 22sccm and oxygen flow rate 20sccm, turn on the planar target sputtering coating power supply, the voltage is 450V, the current is 2.5A, and the coating time is 1200s; during coating, the negative bias voltage is -100V and the coating temperature is 130℃.
[0059] A wear-resistant, blue composite film layer can be obtained.
[0060] In this embodiment, the metal transition layer is 23 nm, the AlFeCrNiCo high entropy alloy layer is 78 nm, and the AlFeCrNiCo high entropy alloy oxide layer is 65 nm.
[0061] Figure 2 It is shown that the composite film layer prepared in this embodiment presents a blue color. According to the measurement, in this embodiment, the LAB value of the AlFeCrNiCo high entropy alloy oxide layer is L: 23.89, a: -3.89b: -24.29.
[0062] Figure 3 The scanning electron microscope photograph of the AlFeCrNiCo high entropy alloy oxide layer of the composite film layer prepared in this embodiment is shown. Figure 3 It can be seen that due to the different values of the atomic radius of cobalt, chromium, iron, nickel and aluminum, the film layer deposited on the substrate after sputtering forms a "yellow beans filling mung beans" effect, thereby giving the film layer density and wear resistance.
[0063] In addition, the atomic percentage of each element in the oxide layer of the AlFeCrNiCo high entropy alloy was obtained through SEM photos, including 10.1% Al, 9.26% Fe, 15.5% Cr, 11.8% Ni, 10.3% Co, 29.2% O, and other elements such as 13.6% C and 0.27% Si.
[0064] Example 2
[0065] The preparation method is basically the same as that in Example 1, except that the argon flow rate is 22 sccm and the oxygen flow rate is 60 sccm in the preparation of the high entropy alloy oxide layer, the planar target sputtering coating power supply is turned on, the voltage is 350 V, the current is 2.0 A, and the coating time is 1800 s; the negative bias voltage during coating is -100 V, and the coating temperature is 100°C.
[0066] According to the measurement, in this embodiment, the LAB value of the AlFeCrNiCo high entropy alloy oxide layer is L: 19.30, a: -2.89b: -25.07. This also shows that the AlFeCrNiCo high entropy alloy oxide layer in this embodiment is blue.
[0067] Example 3
[0068] The preparation method is basically the same as that in Example 1, except that the argon flow rate is 22 sccm and the oxygen flow rate is 30 sccm in the preparation of the high entropy alloy oxide layer, the planar target sputtering coating power supply is turned on, the voltage is 600 V, the current is 5.0 A, and the coating time is 600 s; the negative bias voltage during coating is -200 V, and the coating temperature is 200°C.
[0069] According to the measurement, in this embodiment, the LAB value of the AlFeCrNiCo high entropy alloy oxide layer is L: 26.39, a: -3.27b: -23.21. This also shows that the AlFeCrNiCo high entropy alloy oxide layer in this embodiment is blue.
[0070] Comparative Example 1
[0071] The TiO2 blue optical film layer was prepared by conventional physical vapor deposition process.
[0072] 1. Pre-treat the substrate
[0073] The pretreatment process includes: grinding and polishing the substrate surface, then ultrasonically washing with acetone, deionized water and alcohol and then drying.
[0074] 2. Preparation of TiO2 blue optical film
[0075] The target material is installed in the PVD coating chamber, and two titanium targets are plated in a row by multi-arc ion plating. The pretreated substrate is placed in the vacuum coating machine, and the metal Ti transition layer and the TiO2 blue optical film layer are sputtered in sequence.
[0076] Preparation of titanium transition layer:
[0077] Use titanium target to pre-evacuate the coating chamber to a vacuum degree of 6×10 -3 Pa, argon gas flow rate 20sccm, gas pressure maintained at 3×10 -1 Pa; turn on the multi-arc ion plating power supply, the voltage is 23V, the current is 75A, and the plating time is 120s; during plating, the negative bias voltage is -200V, and the plating temperature is 130℃.
[0078] Preparation of TiO2 blue optical film:
[0079] Use a titanium target and pre-evacuate the coating chamber to a vacuum degree of 6×10 -3 Pa, the oxygen flow rate was 90 sccm, and the pressure was maintained at 4.5×10 -1 Pa; turn on the multi-arc ion plating power supply, the voltage is 23V, the current is 75A, and the plating time is 120s; during plating, the negative bias voltage is -200V, and the plating temperature is 150℃.
[0080] Comparative Example 2
[0081] 1. Pretreatment of substrate:
[0082] The substrate was cleaned with double pure water at room temperature for 480 seconds; the substrate was degreased with ultrasonic wave, wherein the degreasing powder concentration was 55±5g / L, the temperature was 60±10℃, the time was 480 600 seconds, and the ultrasonic current was 2±1A; finally, the substrate was cleaned again with quintuple pure water at room temperature for 1200 seconds.
[0083] 2. Preparation of blue organic coating
[0084] Prepare a blue organic coating. Primer: main agent (white epoxy primer), epoxy reactive diluent (alcohol ether solvent), epoxy resin curing agent (acid anhydride curing agent) = 10:1:(11±1); topcoat: main agent (Lantu high concentration pure white LT-01-1 topcoat 95% + Paint Supervisor C-120 1K standard blue 5%), diluent (alcohol ether solvent), curing agent (acid anhydride curing agent) = 4:1:(3±1).
[0085] The obtained blue organic coating was sprayed on the substrate. The spraying process conditions were: voltage 80KV, air pressure 6kg / cm, paint amount 25cc / min; leveling: line speed 1.5m / min, 25min; curing: temperature 80℃, line speed 1.5m / min, 60min.
[0086] Performance Testing
[0087] The test was carried out according to the provisions of Appendix D of QB / T 5419-2019. The test results are shown in Table 1 below:
[0088] Table 1
[0089]
[0090] As can be seen from the results of Table 1, the friction resistance tests of Examples 1-3 of the present application are all greater than 5000 cycles, indicating that the prepared coating is dense and wear-resistant, giving full play to the excellent properties of high entropy alloys such as high strength / hardness, high toughness, and high wear resistance to improve the various properties of the coating. The adhesion strength test can meet the standard requirements. From the LAB value of the sample appearance, it can be seen that its color change is small, the color difference is small, the process window is stable, and it is suitable for mass production.
[0091] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of protection of this application shall still be based on the scope defined in the attached claims.
Claims
1. A composite film layer, characterized in that: include: Base material; a transition metal layer, which is located on the substrate and is formed by an ion plating method based on a first target in a vacuum environment containing an inert gas; An AlFeCrNiCo high entropy alloy layer, which is located on the transition metal layer and is formed by a sputtering coating method based on a second target in a vacuum environment containing an inert gas; and An AlFeCrNiCo high entropy alloy oxide layer, which is located on the AlFeCrNiCo high entropy alloy layer and is formed by a sputtering coating method based on the second target in a vacuum environment containing an inert gas and oxygen; wherein the first target material is formed of one or more of metals Zr, Ti and Cr; The second target is formed by powder metallurgy using metal powders of Al, Fe, Cr, Ni and Co in an atomic percentage of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.
1.
2. The composite film layer according to claim 1, characterized in that: The second target is formed of metal powders of Al, Fe, Cr, Ni and Co in an atomic percentage of 1:1:1:1:1 by powder metallurgy.
3. The composite film layer according to claim 1 or 2, characterized in that: The thickness of the transition metal layer is in the range of 10 nm to 50 nm, the thickness of the AlFeCrNiCo high entropy alloy layer is in the range of 50 nm to 100 nm, and the thickness of the AlFeCrNiCo high entropy alloy oxide layer is in the range of 50 nm to 100 nm.
4. The composite film layer according to claim 1 or 2, characterized in that: The LAB values of the AlFeCrNiCo high entropy alloy oxide layer are L=23±4, a=-3±1 and b=-24±2.
5. A method for preparing a composite film layer, characterized in that: The method comprises the following steps: 1) placing a pretreated substrate, at least one first target material, and at least one second target material in a coating machine; 2) evacuating the coating machine and continuously introducing an inert gas, turning on a first power source corresponding to the first target material, and forming a metal transition layer on the substrate by an ion plating method; 3) turning off the first power supply and turning on a second power supply corresponding to the second target material, and forming an AlFeCrNiCo high entropy alloy layer on the metal transition layer by a sputtering coating method; and 4) continuously introducing oxygen into the coating machine, and forming an AlFeCrNiCo high entropy alloy oxide layer on the AlFeCrNiCo high entropy alloy layer by a sputtering coating method, thereby obtaining the composite film layer; The first target material is formed of one or more of metals Zr, Ti, and Cr; The second target is formed by powder metallurgy using metal powders of Al, Fe, Cr, Ni and Co in an atomic percentage of 0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.1:0.9-1.
1.
6. The method according to claim 5, characterized in that Step 2) also includes setting the vacuum degree to 8×10 -4 ~6×10 -3 Pa, the flow rate of the inert gas is set in the range of 20 to 60 sccm, and the pressure in the coating machine is maintained at 8×10 -2 ~7×10 -1 Within the range of Pa.
7. The method according to claim 5, characterized in that Step 4) further includes applying a bias voltage of -100 to -200 V to the substrate, the metal transition layer, and the AlFeCrNiCo high entropy alloy layer, and maintaining the pressure in the coating machine at 8×10 -2 ~7×10 -1 Pa range, the coating temperature is set at 100℃~200℃, the coating time is set at 600~1800s, the voltage is set at 350~600V, the current is set at 2~5A, and the argon flow rate is 20~60sccm and the oxygen flow rate is 20~60sccm.
8. A sanitary ware having a composite film layer, characterized in that: The composite membrane layer is a composite membrane layer according to any one of claims 1 to 4 or is prepared by a method according to any one of claims 5 to 7.
Citation Information
Patent Citations
Variable band gap AlCoCrFeNi high-entropy alloy oxide semiconductor film and preparing method thereof
CN108359939A
AlCrNbSiTi high-entropy alloy oxide insulating film material for transistor and preparation method
CN111489956A
Dispersion-strengthened high-entropy alloy nitride ceramic coating with gradient structure and preparation method of dispersion-strengthened high-entropy alloy nitride ceramic coating
CN117187747A
High-entropy alloy powder treatment method and application of treated material thereof
CN117620159A
Method, apparatus and program for consistency checks among multiple manufacturing process equipments using minimum, maximum, and median values of sensor data
KR102830971B1