Perovskite single crystal, preparation method and preparation system thereof, and high-energy ray detector

By compensating vacant defects in perovskites, combined with gradient temperature zone purification and annealing treatment, the problems of easy cracking and high defect density of perovskite single crystals grown in Bridgeman method are solved, and high resistivity and A perovskite single crystal with low defect density, suitable for high-energy ray detectors.

CN119061462APending Publication Date: 2024-12-03BEIJING HAMAMATSU PHOTON TECH INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096508.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing Bridgeman melt method of growing perovskite semiconductor crystals is prone to cracking, poor single crystalline properties and defects due to problems such as insufficient raw material purity, large temperature fluctuations in the growth process, and saturated vapor pressure of Br elements. High density and weak carrier migration ability.

Method used

By determining the target element with a high probability of forming vacancy in perovskites as the second raw material, compensating for vacancy defects, the Bridgeman method is used to grow perovskite single crystals, combined with gradient temperature zone purification and annealing treatment, the quality of the crystal is improved. and performance.

Benefits of technology

Effectively reduce or eliminate vacancy defects, obtain high resistivity, low defect density, and large-size perovskite single crystals, suitable for high-energy ray detectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061462A_ABST
    Figure CN119061462A_ABST
Patent Text Reader

Abstract

The invention provides a perovskite single crystal, a preparation method and a preparation system thereof, and a high-energy ray detector. The preparation method comprises the following steps: taking a raw material prepared according to basic elements contained in a perovskite chemical formula and a stoichiometric ratio of the basic elements as a first raw material; determining a target element from the basic elements according to the probability that each basic element forms a vacancy in the perovskite; the probability that the target element forms vacancies in the perovskite is not less than the probability that other elements form vacancies in the perovskite; taking a raw material consisting of target elements as a second raw material; and preparing the perovskite single crystal based on the first raw material and the second raw material. According to the invention, the second raw material composed of the target elements with relatively high probability of forming vacancies in perovskite is added, so that the formed vacancies can be compensated in the growth process of the perovskite single crystal, the vacancy defect can be effectively reduced or eliminated, and the perovskite single crystal with high resistivity, low defect density and large size can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a perovskite single crystal, and in particular, to a perovskite single crystal and a preparation method and system thereof, and a high-energy ray detector. Background Art

[0002] Nuclear radiation detection is a major national strategic need and has extremely important applications in nuclear safety, nuclear medicine, and nuclear environmental protection. Since the discovery of cadmium zinc telluride (CZT) crystals, research on new room-temperature radiation detectors and radiation detection materials has progressed rapidly. CZT crystals have high melting points (1000-1300°C) and are prone to defects such as inclusions, resulting in high production costs and low yields. Perovskite semiconductor crystals have a carrier-mobility lifetime product (μτ:10 -2 ~10 -3 cm 2 ·V -1 ), high resistivity (10 9 ~10 11 It has become the research focus in the field of direct detection due to its excellent properties such as high Ωcm) and irradiation stability, and is widely studied as the next generation of room temperature radiation detection materials to replace CZT and TlBr.

[0003] In the field of high-energy radiation detection, with the development of the electronics and semiconductor industries, direct detection based on semiconductor crystals has significantly improved detection performance compared to indirect detection based on scintillators because of its good time characteristics and high spatial resolution. In recent years, research on perovskite semiconductor crystals in the field of radiation detection has gradually increased. Studies have shown that perovskite semiconductor crystals have great potential for use in photon counting detectors and photon counting CT.

[0004] There are two main methods for growing perovskite semiconductor single crystals: solution method and melt method. There is an existing technology that uses a low-temperature solution method to successfully prepare CsPbBr3 single crystals with a size of centimeters. However, although the solution method can effectively reduce the growth temperature, the size of the crystal is much smaller than that of the crystal grown by the melt method, and the performance index is also lower than that of the crystal grown by the melt method. The melt method, especially the Bridgman method, is a universal method for batch growth of low defect density and large-sized bulk single crystals. It has the potential to be used for the growth of large-sized, high-quality perovskite semiconductor single crystals. In recent years, there have been some reports on the growth of perovskite single crystals using the Bridgman method.

[0005] CN110219046A and CN110923813A disclose the use of a vertical Bridgman method to grow a CsPbBr3 single crystal and mixed halide perovskite single crystal CsPbBr 3-n X n(X=Cl, I) technology, CN105483825A, CN108193271A, CN109112627A disclose the use of vertical Bridgman method, horizontal moving zone melting method and electric controlled dynamic gradient solidification method to grow CsPbBr3, and conduct X-ray and γ-ray detection performance tests and element doping research. The size of the grown CsPbBr3 crystal is CN 115710744A discloses a series of AB1B2X type large size crystals grown by descending crystallization by the Bridgman method. Double perovskite crystal.

[0006] However, the perovskite semiconductor crystals currently grown by the Bridgman melt method have problems such as insufficient raw material purity, large fluctuations in the temperature field of the growth process, and high saturated vapor pressure of the Br element, which leads to problems such as easy cracking of large-sized crystals, poor single crystallinity, high defect (vacancy) density, and weak carrier migration ability. Summary of the invention

[0007] In order to solve at least one of the above existing technical problems, the first aspect of the present application provides a method for preparing a perovskite single crystal. The preparation method comprises:

[0008] Using a raw material prepared according to the basic elements included in the perovskite chemical formula and the stoichiometric ratio between the basic elements as a first raw material;

[0009] Determining a target element from the basic elements according to the probability of each basic element forming a vacancy in the perovskite; wherein the probability of the target element forming a vacancy in the perovskite is not less than the probability of other elements forming a vacancy in the perovskite;

[0010] Using a raw material composed of the target element as a second raw material; and

[0011] A perovskite single crystal is prepared based on the first raw material and the second raw material.

[0012] In some embodiments of the present application, the second raw material is 2-5 wt % of the total amount of the first raw material.

[0013] In some embodiments of the present application, according to the probability of each basic element forming a vacancy in the perovskite, determining the target element from the basic elements includes:

[0014] Sort the basic elements in ascending or descending order according to the probability of forming vacancies in the perovskite, and select the elements in the first N positions in descending order or the last N positions in ascending order from the basic elements as target elements, where N is an integer greater than or equal to 2;

[0015] Optionally, the target element includes a halogen and at least one monovalent, divalent or trivalent ion; using a raw material composed of the target element as the second raw material comprises:

[0016] A compound consisting of halogen and other target elements is used as the second raw material.

[0017] In some embodiments of the present application, when the chemical formula of the perovskite is ABX3, the target element includes B and X, and the second raw material includes BX2; wherein the A ion includes Rb + and / or Cs + , B ions include Sn 2+ and / or Pb 2+ , X ions include Cl – Br – and I – One or more of; or

[0018] When the chemical formula of the perovskite is A2B Ⅰ B Ⅲ When X6, the target elements include X and B Ⅰ and / or B Ⅲ The second raw material includes B Ⅰ X and / or B Ⅲ X3; where A ions include Rb + and / or Cs + , B Ⅰ Ions include Li + 、Na + , K + , Rb + 、Ag + One or more of B Ⅲ Ions include Al 3+ , Ga 3+ 、In 3+ , Tl 3+ 、Bi 3+ , Sb 3+ One or more of the X ions include Cl – Br – and I – One or more of .

[0019] In some embodiments of the present application, preparing a perovskite single crystal based on the first raw material and the second raw material includes:

[0020] synthesizing the first raw material into a perovskite polycrystalline material;

[0021] Purifying the perovskite polycrystalline material; and

[0022] The perovskite single crystal is generated by using the perovskite polycrystalline material and the second raw material.

[0023] In some embodiments of the present application, purifying the perovskite polycrystalline material includes:

[0024] Keeping the perovskite polycrystalline material warm in a first temperature zone having a first temperature until the perovskite polycrystalline material is melted;

[0025] Moving the melted perovskite polycrystalline material from the first temperature zone to a second temperature zone having a second temperature; wherein a gradient temperature zone is provided between the first temperature zone and the second temperature zone; and

[0026] Removing impurities accumulated at the tail end of the perovskite polycrystalline material;

[0027] Optionally, the first temperature is 20°C to 100°C higher than the melting point of the perovskite single crystal, and the second temperature is 20°C to 100°C lower than the melting point of the perovskite single crystal;

[0028] Optionally, the temperature gradient of the gradient temperature zone is 30-50° C. / cm.

[0029] In some embodiments of the present application, the moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 3 to 20 mm / h, or the moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 10 to 20 times the descending speed when the perovskite single crystal is grown by the Bridgman method.

[0030] In some embodiments of the present application, generating the perovskite single crystal by using the perovskite polycrystalline material and the second raw material includes:

[0031] Putting the seed crystal for inducing the growth of the perovskite single crystal, the second raw material and the perovskite polycrystalline material into the first crucible in order from bottom to top;

[0032] placing the first crucible into a first furnace body, and growing a perovskite single crystal by a Bridgman method;

[0033] Optionally, the descending speed when growing the perovskite single crystal by the Bridgman method is 0.3-1 mm / h.

[0034] In some embodiments of the present application, the preparation method further comprises:

[0035] Annealing the perovskite single crystal;

[0036] Optionally, the annealing temperature is 250-350° C., and the annealing time is 6-14 h;

[0037] Optionally, after annealing is completed, the perovskite single crystal is cooled to room temperature at a rate of 10 to 30° C. / h.

[0038] A second aspect of the present application provides a system for preparing a perovskite single crystal, comprising:

[0039] A first crucible includes a first body for containing a first raw material and a second raw material; wherein the first raw material is a raw material prepared according to the basic elements included in the perovskite chemical formula and the stoichiometric ratio between the basic elements, and the second raw material is a raw material composed of a target element, wherein the target element is a target element determined from the basic elements according to the probability of each basic element forming a vacancy in the perovskite, and the probability of the target element forming a vacancy in the perovskite is not less than the probability of other elements forming a vacancy in the perovskite; and

[0040] The first furnace body is used to accommodate the first crucible and provide a required temperature environment for preparing a perovskite single crystal based on the first raw material and the second raw material.

[0041] In some embodiments of the present application, the first furnace body includes a furnace cavity for accommodating the first crucible;

[0042] A first bottom support for supporting the first crucible is arranged in the furnace chamber, and the first bottom support and the first crucible are connected via a metal rod with heat conduction function;

[0043] Optionally, a water-cooling rod that penetrates the furnace cavity and can move up and down in the furnace cavity is connected to the bottom of the first base, and a lifting control mechanism is connected to the bottom of the water-cooling rod to control the water-cooling rod to drive the first crucible to move in the furnace cavity.

[0044] In some embodiments of the present application, the metal rod is made of one or more of silver, aluminum, copper, and zinc.

[0045] In some embodiments of the present application, a first heating element, a second heating element, and a heat insulation board located between the first heating element and the second heating element are disposed on the side wall of the furnace cavity;

[0046] wherein the first heating element can form a first temperature zone in the first furnace body after being heated, the second heating element can form a second temperature zone in the first furnace body after being heated, and the heat insulation board can form a gradient temperature zone in the first furnace body after the first heating element and the second heating element are heated;

[0047] Optionally, the height of the first temperature zone is 250-350 mm, the height of the gradient temperature zone is 20-30 mm, and the height of the second temperature zone is 150-250 mm.

[0048] The third aspect of the present application provides a perovskite single crystal, which is obtained by any of the above-mentioned preparation methods or any of the above-mentioned preparation systems.

[0049] A fourth aspect of the present application provides a high-energy ray detector, which includes the above-mentioned perovskite single crystal;

[0050] Optionally, the resistivity of the high-energy ray detector is 5 to 9×10 10 Ω·cm;

[0051] Optionally, the high energy ray detector is 137 The energy resolution of the 662keV gamma rays emitted by Cs is 2-3%.

[0052] The present application adds a second raw material composed of a target element with a high probability of forming vacancies in perovskite during the growth process of the perovskite single crystal, thereby being able to compensate for the vacancies formed during the growth process of the perovskite single crystal, and being able to effectively reduce or eliminate vacancy defects, thereby being able to obtain a perovskite single crystal with high resistivity, low defect density, and large size.

[0053] The preparation system provided in the present application inserts a metal rod with good thermal conductivity under the bottom support of the crucible. During the crystal growth process, it can enhance the extraction effect of the crystallization latent heat at the seed crystal position and the center position of the ingot, thereby obtaining an ideal micro-convex interface for single crystal growth.

[0054] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] The following is a detailed description of the implementation methods of the present application in conjunction with the accompanying drawings. Here, the accompanying drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application.

[0056] Figure 1 The figure shows a process flow for preparing a perovskite single crystal provided in one embodiment of the present application.

[0057] Figure 2 The process flow of preparing perovskite single crystal based on the first raw material and the second raw material provided in one embodiment of the present application is shown.

[0058] Figure 3 A vertical Bridgman descending furnace for growing perovskite single crystals in a perovskite single crystal preparation system provided in an embodiment of the present application is shown.

[0059] Figure 4A vertical Bridgman descending furnace for purifying perovskite polycrystals in a perovskite single crystal preparation system provided in an embodiment of the present application is shown. DETAILED DESCRIPTION

[0060] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.

[0061] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0062] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or mutual communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0063] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply means that the first feature is lower in level than the second feature.

[0064] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.

[0065] The preferred embodiments of the present application are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present application and are not used to limit the present application.

[0066] Figure 1 A method for preparing a perovskite single crystal provided in an embodiment of the present application is shown, comprising the following steps S1 to S4.

[0067] S1: Raw materials prepared according to the basic elements included in the chemical formula of perovskite and the stoichiometric ratios of the basic elements are used as the first raw material.

[0068] Each element in the chemical formula of the perovskite to be prepared is the basic element. For example, the chemical formula of the perovskite to be prepared can be ABX3 or A2B Ⅰ B Ⅲ When preparing a perovskite with a chemical formula of ABX3 (hereinafter referred to as ABX3 perovskite), the basic elements include A, B and X elements, and the first raw material may include AX and BX2. Ⅰ B Ⅲ X6 perovskite (hereinafter referred to as A2B Ⅰ B Ⅲ X6 perovskite), the basic elements include A, B Ⅰ , B Ⅲ and X element, the first raw material may include AX, B Ⅰ X and B Ⅲ X3.

[0069] In the above chemical formula, A ions may include Rb +and / or Cs + , B ions may include Sn 2+ and / or Pb 2+ , B Ⅰ The ions may include Li + 、Na + , K + , Rb + 、Ag + One or more of B Ⅲ Ions may include Al 3+ , Ga 3+ 、In 3+ , Tl 3+ 、Bi 3+ , Sb 3+ One or more of the X ions may include Cl – Br – and I – One or more of .

[0070] When each of the A ions, B ions, and X ions includes only one element, the ABX3 perovskite may be referred to as a ternary perovskite. Ⅰ Ion, B Ⅲ When each of the A2B ions and the X ions consists of only one element, Ⅰ B Ⅲ X6 perovskite can be called a quaternary perovskite. Of course, A ions, B ions, B Ⅰ Ion, B Ⅲ Each of the X ions and the Cl ions may also include multiple elements. For example, the X ions may include Cl – and Br – , or Cl – and I – , or Br – and I – , or Cl – Br – and I – , at this time the perovskite can be called a mixed halide perovskite.

[0071] In order to ensure the purity of the obtained single crystal, high-purity (eg, ≥5N) raw materials may be used. When weighing the raw materials, the weighing may be performed in a dry glove box.

[0072] S2: Determine the target element from the basic elements according to the probability of each basic element forming a vacancy in the perovskite.

[0073] S3: Using a raw material composed of the target element as the second raw material.

[0074] Among them, the probability of the target element forming a vacancy in the perovskite is not less than the probability of other elements forming a vacancy in the perovskite.

[0075] During the growth of perovskite, due to the high saturated vapor pressure of halogen elements, they are easily diffused into the free space inside the crucible, resulting in halogen ion vacancy defects inside the crystal. Halogen ion vacancy defects are the cause of ion migration during the use of perovskite crystals, leading to detector polarization.

[0076] In order to reduce or eliminate vacancy defects, the present application adds a second raw material composed of a target element during the preparation of a perovskite single crystal. Since the probability of the selected target element forming a vacancy in the perovskite is greater than or equal to the probability of other elements forming a vacancy in the perovskite, the vacancy formed can be compensated during the growth of the perovskite single crystal, and the vacancy defects can be effectively reduced or eliminated.

[0077] Optionally, step S2 includes: sorting each basic element in ascending or descending order according to the probability of forming a vacancy in the perovskite, and selecting the element ranked in the first N positions in descending order or the last N positions in ascending order from the basic elements as the target element, wherein N is an integer greater than or equal to 2. At this time, several elements with a higher probability of forming a vacancy in the perovskite can be conveniently selected by sorting.

[0078] Optionally, the target element includes a halogen and at least one monovalent, divalent or trivalent ion. Step S3 may include: using a compound composed of a halogen and other target elements as a second raw material. At this time, halogen is generally the element with the highest probability of forming a vacancy in perovskite, so the target element includes a halogen, and the target element also includes another one or more elements, so that the compound composed of the halogen and the halogen is used as the second raw material. Among them, the other one or more elements can be selected based on the results of the sorting in step S2, and may include at least one monovalent, divalent or trivalent ion.

[0079] For example, for ABX3 perovskite, after sorting in step S2, the probability of B ions and halogen X ions forming vacancies in the perovskite is greater than that of A ions. In this case, the target elements are selected as B and X, and the second raw material is BX2. In some specific embodiments, the second raw material can be one or more of SnCl2, SnBr2, SnI2, PbCl2, PbBr2 and PbI2. Ⅰ B Ⅲ For X6 perovskite, after sorting in step S2, B Ⅰ Ion, B Ⅲ The probability of A ions and X ions forming vacancies in perovskite is greater than that of A ions. In this case, the target elements can be X and B Ⅰ and / or B Ⅲ, the second raw material can be B Ⅰ X and / or B Ⅲ X3. In some specific embodiments, the second raw material may be one or more of LiCl, NaCl, KCl, RbCl, AgCl, LiBr, NaBr, KBr, RbBr, AgBr, LiI, NaI, KI, RbI, AgI, AlCl3, GaCl3, InCl3, TlCl3, BiCl3, SbCl3, AlBr3, GaBr3, InBr3, TlBr3, BiBr3, SbBr3, AlI3, GaI3, InI3, TlI3, BiI3 and SbI3.

[0080] In the present application, optionally, the second raw material is 2 to 5 wt% of the total amount of the first raw material. At this dosage, the ions in the second raw material can effectively reduce or eliminate vacancy defects, and they are all constituent elements of the perovskite itself, and no additional impurities are added, so the quality of the obtained perovskite single crystal is very good. In some specific embodiments, the second raw material can be 2 wt%, 2.2 wt%, 2.4 wt%, 2.6 wt%, 2.8 wt%, 3 wt%, 3.2 wt%, 3.4 wt%, 3.6 wt%, 3.8 wt%, 4 wt%, 4.2 wt%, 4.4 wt%, 4.6 wt%, 4.8 wt% or 5 wt% of the first raw material.

[0081] S4: preparing a perovskite single crystal based on the first raw material and the second raw material.

[0082] Optionally, this step includes the following sub-steps S41 to S43: Figure 2 shown.

[0083] S41: synthesizing the first raw material into a perovskite polycrystalline material.

[0084] Optionally, sub-step S41 is performed in a synthesis crucible. The first raw material weighed in step S1 can be placed in a clean synthesis crucible, and then the crucible is evacuated to a certain pressure (e.g., 5×10 -4 Pa or less), then sinter and seal, and place in a synthesis furnace for synthesis.

[0085] Optionally, during the synthesis process, the temperature of the crucible can be first raised to a temperature higher than the raw material with the highest melting point in the first raw material, so that the raw material with the highest melting point can be fully overheated, and the raw material is fully melted, convected, and mixed, thereby avoiding the generation of inclusion phases, which is beneficial to improving the quality of the obtained perovskite polycrystalline material. After the raw materials are fully melted and mixed evenly, the temperature can be cooled to a suitable reaction temperature, and then reacted at this temperature, and kept warm for a period of time, so that the first raw material reacts completely. After the reaction is completed, the temperature can be slowly cooled to room temperature to obtain a perovskite polycrystalline material. The polycrystalline material obtained by the above method is of good quality.

[0086] For example, for ABX3 perovskite, the first raw materials are AX and BX2, and the raw material with the highest melting point is AX. When heating up the synthesis, first raise the temperature of the synthesis furnace to a temperature higher than the melting point of AX, wait for AX to completely melt, then cool it down to a suitable reaction temperature, and then keep it warm for a period of time to allow AX and BX2 to fully react and generate ABX3 perovskite polycrystalline material. Ⅰ B Ⅲ X6 perovskite, the first raw material is AX, B Ⅰ X and B Ⅲ X3, at this time the raw material with the highest melting point is also AX. When heating up the synthesis, first raise the temperature of the synthesis furnace to a temperature higher than the melting point of AX, wait until AX is completely melted, then cool it down to a suitable reaction temperature, and then keep it warm for a period of time, so that AX, B Ⅰ X and B Ⅲ X3 fully reacts to generate A2B Ⅰ B Ⅲ X6 perovskite polycrystalline material.

[0087] S42: Purifying the perovskite polycrystalline material.

[0088] The polycrystalline material generated above contains impurities. In order to remove these impurities, the present application purifies the perovskite polycrystalline material.

[0089] The purification method may include the following steps: keeping the perovskite polycrystalline material in a first temperature zone having a first temperature until the perovskite polycrystalline material melts; and moving the melted perovskite polycrystalline material from the first temperature zone to a second temperature zone having a second temperature. That is, after the perovskite polycrystalline material is melted, in the process of the melted perovskite polycrystalline material moving from the first temperature zone to the second temperature zone, due to the change in temperature, the perovskite polycrystalline material will gradually solidify from one end close to the first temperature zone, and the impurities are "moved" to the tail end of the polycrystalline material to form a segregation layer by utilizing the different solubility of impurities in the melt and the solid, and then the segregation layer can be removed.

[0090] Among them, a gradient temperature zone is provided between the first temperature zone and the second temperature zone. The temperature of the first temperature zone is higher, and the temperature of the second temperature zone is slightly lower. Optionally, the first temperature is 20°C to 100°C higher than the melting point of the perovskite single crystal, and the second temperature is 20°C to 100°C lower than the melting point of the perovskite single crystal. For example, the temperature of the first temperature zone can be set to 460 to 480°C, and the temperature of the second temperature zone can be set to 250 to 300°C. Optionally, the temperature gradient of the gradient temperature zone is 30 to 50°C / cm. The gradient temperature zone provides a larger temperature gradient, which can promote the "movement" of impurities and achieve better impurity removal effect. The gradient temperature zone can be achieved by setting a heat insulation board between the first temperature zone and the second temperature zone.

[0091] In some specific embodiments, the first temperature may be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C higher than the melting point of the perovskite single crystal. In some specific embodiments, the second temperature may be 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C lower than the melting point of the perovskite single crystal. In some specific embodiments, the temperature gradient of the gradient temperature zone may be 30°C / cm, 32°C / cm, 34°C / cm, 36°C / cm, 38°C / cm, 40°C / cm, 42°C / cm, 44°C / cm, 46°C / cm, 48°C / cm or 50°C / cm.

[0092] Optionally, the moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 3 to 20 mm / h, or the moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 10 times / 10 times or more to 20 times / 20 times or less (10 to 20 times) the descent speed when the perovskite single crystal is grown by the Bridgman method. At this speed, it has a good purification effect and can significantly improve the efficiency of polycrystalline material purification. However, the descent speed cannot be excessively increased, and a too fast descent will cause the purification effect to continue to weaken.

[0093] In some specific embodiments, the moving speed may be 3 mm / h, 5 mm / h, 7 mm / h, 9 mm / h, 10 mm / h, 12 mm / h, 14 mm / h, 16 mm / h, 18 mm / h or 20 mm / h. In other specific embodiments, the moving speed may be 11 times, 12 times, 13 times, 14 times, 15 times, 16 times, 17 times, 18 times, 19 times or 20 times the descending speed when the perovskite single crystal is grown by the Bridgman method.

[0094] Optionally, the present application adopts the method of rapidly moving the aforementioned polycrystalline material from the top to the bottom in a vertical Bridgman descending furnace to purify the polycrystalline material, which is referred to as the "rapid Bridgman descending method" in the present application. The method may specifically include: placing the perovskite polycrystalline material in a purification crucible; heating the first temperature zone of the vertical Bridgman descending furnace to a first temperature, and heating the second temperature zone of the vertical Bridgman descending furnace to a second temperature; and placing the purification crucible containing the perovskite polycrystalline material in the first temperature zone, and descending the purification crucible from the first temperature zone to the second temperature zone at the aforementioned moving speed (3 to 20 mm / h or 10 to 20 times the descending speed when growing a perovskite single crystal). The first temperature zone and the second temperature zone in the vertical Bridgman descending furnace can be heated by heating elements, and the gradient temperature zone can be formed by arranging a heat insulation plate between the heating elements.

[0095] The method provided by the present application utilizes the difference in solubility of impurities in the solid and liquid phases of the material, so that the impurities in the polycrystalline material gradually "move" from the crystallized part to the molten part during the descent of the crucible, and finally enriched at the tail end of the perovskite polycrystalline material. In this method, the "faster descent speed" and "larger temperature gradient" work together to improve the purification efficiency while ensuring the purification effect. Purification can be carried out multiple times or only once, depending on actual needs. After purification, the polycrystalline material can be cooled to room temperature with the furnace, and then the impurities at the tail end of the polycrystalline material can be removed.

[0096] S43: generating a perovskite single crystal using the perovskite polycrystalline material and the second raw material.

[0097] Optionally, this step adopts a seed crystal induction method to grow a perovskite single crystal. The crystal grown by this method has high purity.

[0098] Optionally, this step includes: placing a seed crystal for inducing the growth of a perovskite single crystal, a second raw material and a perovskite polycrystalline material into a first crucible in order from bottom to top; and placing the first crucible into a first furnace body to grow a perovskite single crystal using a Bridgman method.

[0099] Here, the seed crystal, the second raw material and the perovskite polycrystalline material need to be placed in the first crucible in order from bottom to top. The cone of the first crucible is provided with a seed crystal container, so that the seed crystal can play a good inducing role and guide the directional growth of the single crystal, and the second raw material can effectively compensate for the vacancy defects during the growth of the single crystal. After the seed crystal, the second raw material and the perovskite polycrystalline material are placed in the first crucible, it is necessary to evacuate (for example, evacuate to 5×10 -4 Pa or less) and sinter the sealed crucible.

[0100] The process of growing perovskite single crystals using the Bridgman method may include: first, placing a first crucible containing the aforementioned materials into a vertical Bridgman descending furnace (first furnace body) for heating, so that the perovskite polycrystalline material is completely melted and the seed crystal is partially melted, and then lowering the first crucible from top to bottom in the vertical Bridgman descending furnace (first furnace body), thereby growing the perovskite single crystal and allowing the target element to be doped into the perovskite single crystal.

[0101] Optionally, the vertical Bridgman descending furnace (first furnace body) used to grow perovskite single crystals is the same as the vertical Bridgman descending furnace used to purify perovskite polycrystals, but the crucibles and corresponding bases used are different. The base of the first furnace body is adapted to the cone of the first crucible, the cone of the first crucible is provided with a columnar tail for accommodating the seed crystal, and the base of the first furnace body is provided with a portion for accommodating the columnar tail. Furthermore, a metal rod with good thermal conductivity can be arranged between the base of the first furnace body and the first crucible, which can enhance the extraction effect of the crystallization latent heat at the seed crystal position and the center of the ingot during the crystal growth process, thereby obtaining an ideal micro-convex interface for single crystal growth. For the specific structure of the first furnace body, please refer to the introduction of the preparation system of the perovskite single crystal below, which will not be repeated here.

[0102] Of course, the vertical Bridgman descending furnace (first furnace body) used for growing perovskite single crystals and the vertical Bridgman descending furnace used for purifying perovskite polycrystals can also be different, as long as they can complete the growth of perovskite and the purification of perovskite polycrystals.

[0103] When growing a perovskite single crystal, the temperatures of the first temperature zone and the second temperature zone of the vertical Bridgman descending furnace (first furnace body) are different from the temperatures of the first temperature zone and the second temperature zone of the vertical Bridgman descending furnace when purifying perovskite polycrystals. In some specific embodiments, when growing a perovskite single crystal, the temperatures of the first temperature zone and the second temperature zone of the vertical Bridgman descending furnace may be 470-500°C and 380-400°C, respectively. For example, when growing a perovskite single crystal, the temperature of the first temperature zone of the vertical Bridgman descending furnace may be 470°C, 475°C, 480°C, 485°C, 490°C, 495°C or 500°C. For example, when growing a perovskite single crystal, the temperature of the second temperature zone of the vertical Bridgman descending furnace may be 380°C, 385°C, 390°C, 395°C or 400°C. In some specific embodiments, the maximum temperature gradient in the central area of ​​the heat insulation board can reach 30°C / cm, and the larger temperature gradient provides sufficient driving force for the growth of the single crystal. For a detailed introduction to the various temperature zones in the first furnace, please refer to the introduction to the preparation system of perovskite single crystals below, which will not be repeated here.

[0104] Optionally, the descent rate when growing the perovskite single crystal by the Bridgman method is 0.3 to 1 mm / h. If the descent rate is too fast, the growth is incomplete, and if the descent rate is too slow, the growth efficiency is low. In some specific embodiments, the descent rate may be 0.3 mm / h, 0.4 mm / h, 0.5 mm / h, 0.6 mm / h, 0.7 mm / h, 0.8 mm / h, 0.9 mm / h or 1 mm / h. Appropriate temperature gradient, descent rate, and cooling rate are conducive to the growth of high-quality single crystals with good single crystallinity, integrity, and transparency.

[0105] Perovskite single crystals grown by the Bridgman method may have antisite defects, especially quaternary perovskites or multi-element perovskites. For example, for CABB crystals (Cs2AgBiBr6), Ag and Bi elements are prone to Ag + / Bi 3+ Disorder phenomenon, some Ag + Occupies Bi 3+ The lattice sites of Bi 3+ Occupies Ag + The antisite defect will make the crystal disordered and lead to the degradation of crystal performance.

[0106] In order to reduce antisite defects, optionally, the method provided in the present application further includes: annealing the perovskite single crystal. Optionally, the annealing temperature is 250 to 350°C, and the annealing time is 6 to 14 hours. Annealing under appropriate temperature conditions can reduce antisite defects and return dislocated atoms to their original positions. In some specific embodiments, the annealing temperature may be 250°C, 270°C, 290°C, 310°C, 330°C or 350°C.

[0107] In the present application, the perovskite single crystal can be annealed in situ, that is, after the crystal growth is completed, the position of the crystal is not moved, and the furnace temperature is adjusted to the annealing temperature for in situ annealing.

[0108] Optionally, after annealing is completed, the perovskite single crystal is cooled to room temperature at a rate of 10 to 30°C / h. A slow cooling rate is conducive to the discharge of thermal stress inside the crystal. In some specific embodiments, the perovskite single crystal can be cooled to room temperature at a rate of 10°C / h, 12°C / h, 14°C / h, 16°C / h, 18°C / h, 20°C / h, 22°C / h, 24°C / h, 26°C / h, 28°C / h or 30°C / h.

[0109] The above method provided in the present application can effectively reduce or eliminate halogen ion vacancy defects, and purifies the polycrystalline material. The obtained perovskite single crystal has high transparency, good integrity, high resistivity and low defect density, and is very suitable for use in high-energy ray detectors.

[0110] Figure 3 A vertical Bridgman descending furnace 100 for growing a perovskite single crystal in a system for preparing a perovskite single crystal provided in an embodiment of the present application is shown. The vertical Bridgman descending furnace 100 includes a first crucible 110 and a first furnace body 120 hereinafter referred to as the first crucible.

[0111] The first crucible 110 includes a first body for containing the first raw material and the second raw material. The first furnace body 120 is used to contain the first crucible 110 and provide a required temperature environment for preparing a perovskite single crystal based on the first raw material and the second raw material.

[0112] The first furnace body 120 includes a furnace cavity for accommodating the first crucible 110 . A first base 131 for supporting the first crucible 110 is disposed in the furnace cavity. The first base 131 and the first crucible 110 are connected via a metal rod 132 with a heat conduction function.

[0113] In the process of growing perovskite single crystals by the Bridgman method, the morphology of the solid-liquid interface is one of the key factors affecting the single crystal rate. A slightly convex or horizontal growth interface is more conducive to obtaining single crystals. The present application inserts a metal rod with good thermal conductivity under the bottom support of the crucible, which can enhance the extraction effect of the crystallization latent heat at the seed crystal position and the center of the ingot during the crystal growth process, thereby obtaining an ideal slightly convex interface for single crystal growth.

[0114] Alternatively, if Figure 3 As shown, the bottom of the first bottom bracket 131 is connected to a water-cooled rod 133 that penetrates the furnace cavity and can move up and down in the furnace cavity. The bottom of the water-cooled rod 133 is connected to a lifting control mechanism 140 for controlling the water-cooled rod 133 to drive the first crucible 110 to move in the furnace cavity. The metal rod 132 can be connected to the water-cooled rod 133, such as Figure 3 As shown, this is more conducive to the metal rod 132 to conduct away the crystallization latent heat at the seed crystal position and the center position of the ingot.

[0115] Optionally, the metal rod is made of one or more of silver, aluminum, copper, and zinc, which have better thermal conductivity.

[0116] Optionally, a first heating element 121, a second heating element 122, and a heat insulation board 123 located between the first heating element 121 and the second heating element 122 are provided on the side wall of the furnace cavity. The first heating element 121 can form a first temperature zone A1 in the first furnace body 120 after being heated, the second heating element 122 can form a second temperature zone A2 in the first furnace body 120 after being heated, and the heat insulation board 123 can form a gradient temperature zone A3 in the first furnace body 120 after the first heating element 121 and the second heating element 122 are heated.

[0117] Optionally, the height of the first temperature zone A1 is 250-350 mm, the height of the gradient temperature zone A3 is 20-30 mm, and the height of the second temperature zone A2 is 150-250 mm. The first temperature zone A1, the second temperature zone A2 and the gradient temperature zone A3 of the above heights can form a suitable large gradient temperature field to provide sufficient driving force for single crystal growth. In some specific embodiments, the height of the first temperature zone A1 may be 250 mm, 270 mm, 290 mm, 310 mm, 330 mm or 350 mm. In some specific embodiments, the height of the gradient temperature zone A3 may be 20 mm, 22 mm, 24 mm, 26 mm, 28 mm or 30 mm. In some specific embodiments, the height of the second temperature zone A2 may be 150 mm, 170 mm, 190 mm, 210 mm, 230 mm or 250 mm.

[0118] When the temperature of the first temperature zone A1 is 470-500°C, the temperature of the second temperature zone A2 is 380-400°C, the maximum temperature gradient in the central area of ​​the gradient temperature zone A3 can reach 30°C / cm, and the temperature gradient change curve above and below the central area basically conforms to the Gaussian distribution. The larger temperature gradient provides sufficient driving force for the growth of the single crystal and is more conducive to the discharge of remaining impurities. Of course, the temperature gradient should not be too large to avoid large thermal stress inside the crystal, which may cause the crystal to crack.

[0119] Figure 3 In the illustrated embodiment, the first body of the first crucible 110 includes, from bottom to top, a cylindrical tail portion 111 for accommodating a seed crystal, an inner cavity 112, and a crucible mouth 113, wherein the cylindrical tail portion 111 and the inner cavity 112 are connected. The diameter of the inner cavity 112 is greater than the diameter of the cylindrical tail portion 111, and the connection portion between the bottom of the inner cavity 112 and the cylindrical tail portion 111 can be designed to be a cone-like structure. Optionally, the first bottom support 131 and the metal rod 132 of the first furnace body 120 are detachably connected to a water cooling device 133, and the water cooling device 133 is detachably connected to a lifting control mechanism 140. The first base 131 can adapt to the bottom setting of the first crucible 110, including a first cone-like structure corresponding to the above-mentioned connecting portion and a second structure corresponding to the cylindrical tail 111. The second structure can accommodate the metal rod 132 and the cylindrical tail 111. The metal rod 132 can provide supporting force to the cylindrical tail 111. The first structure supports the cone-like connecting portion. Figure 3 In the illustrated embodiment, the vertical Bridgman descending furnace 100 further includes a base 150 , and the first furnace body 120 and the lifting control mechanism 140 are disposed on the base 150 and connected to the base 150 . Figure 3 In the embodiment shown, the outer surface of the furnace chamber is provided with a heat-insulating layer. The first crucible 110 may be a quartz crucible.

[0120] In some specific embodiments, the process of growing a perovskite single crystal using the first crucible 110 and the first furnace body 120 may include: 1) heating the first temperature zone A1 and the second temperature zone A2 of the first furnace body 120 to a predetermined temperature; 2) placing a seed crystal processed by precise orientation into the columnar tail 111 of the first crucible 110, and then placing a second raw material on top of the seed crystal, and then placing a perovskite polycrystalline material on top of the second raw material, and then evacuating to a certain pressure, and then sintering and sealing the crucible of the first crucible 110. The crucible 113 is then placed into the first furnace body 120, so that the seed crystal is located in the gradient temperature zone A3, and the perovskite polycrystal is located in the first temperature zone A2; 3) the temperature is kept warm for a certain period of time so that the perovskite polycrystal is fully melted and the seed crystal is partially melted, and then the first bottom support 131 is controlled by the lifting control mechanism 140, so that the first crucible 110 descends from the first temperature zone A1 to the gradient temperature zone A3 and the second temperature zone A2 in sequence at a predetermined rate until the melt is completely crystallized and the single crystal growth is completed, and then the descent stops.

[0121] Optionally, when the vertical Bridgman descending furnace 100 is used to purify perovskite polycrystals, the first base 131 and the metal rod 132 need to be removed and replaced with the second base 161 and the second crucible 170 (also referred to as a purification crucible in this application), such as Figure 4 shown. Figure 4 In the embodiment shown, when purifying perovskite polycrystal, the vertical Bridgman descending furnace 100 includes a second crucible 170, a first furnace body 120, a water cooling device 133, a second bottom support 161, a lifting control mechanism 140, and a base 150. Figure 3 The same structure will not be repeated here.

[0122] The second crucible 170 includes a second body for accommodating the perovskite polycrystalline material. The second crucible 170 can be mounted on the second base 161 for purifying the perovskite polycrystalline material. The second crucible 170 is not provided with a columnar tail for accommodating the seed crystal, and its bottom is a conical structure. The second base 161 is adapted to the shape of the second crucible 170 and is also designed to be a similar conical structure for supporting the second crucible 170. Figure 4 In the illustrated embodiment, the first furnace body 120 and the lifting control mechanism 140 are disposed on the base 150 and are respectively connected to the base 150; no metal rod 132 is disposed between the second bottom support 161 and the second crucible 170, and the second crucible 170 is directly connected to the lifting control mechanism 140 through the water cooling device 133; the first furnace body 120 is used to heat the second crucible 170. Under the action of the lifting control mechanism 140, the second crucible 170 can rise into or descend out of the first furnace body 120, thereby purifying the perovskite polycrystalline material.

[0123] In some specific embodiments, the process of purifying the perovskite polycrystalline using the second crucible 170 and the first furnace body 120 may include: 1) placing the perovskite polycrystalline material in the second crucible 170; 2) heating the first temperature zone A1 and the second temperature zone A2 of the first furnace body 120 to a predetermined temperature; 3) placing the second crucible 170 containing the perovskite polycrystalline material in the first temperature zone A1, and lowering the second crucible 170 from the first temperature zone A1 to the second temperature zone A2, so that impurities are enriched at the tail end of the perovskite polycrystalline material. The specific process can be found in the above description, which will not be repeated here.

[0124] Optionally, the preparation system of the perovskite single crystal provided in the present application also includes a synthesis furnace for synthesizing perovskite polycrystalline material. The synthesis furnace may include a third crucible (also referred to as a synthesis crucible in the present application) and a second furnace body. The third crucible is used to synthesize the perovskite polycrystalline material, and the second furnace body is used to accommodate the third crucible and provide heat for the third crucible. The structure of the third crucible and the second furnace body can refer to the structure of the second crucible 170 and the first furnace body 120.

[0125] Optionally, the cone angle of the third crucible used is 30° to 80°. At this angle, it is beneficial to improve the quality of the synthesized perovskite polycrystalline material. In some specific embodiments, the cone angle of the third crucible used may be 30°, 35°, 40°, 45°, 50°, 55°, 60°, 65°, 70°, 75° or 40°.

[0126] The above-mentioned preparation system provided in the present application can obtain perovskite single crystals with high transparency, good integrity, high resistivity and low defect density, which are very suitable for use in high-energy ray detectors.

[0127] In specific applications, the grown perovskite single crystal can be processed into a wafer of a certain thickness. The processed wafer is subjected to vacuum thermal evaporation to deposit metal electrodes on the upper and lower surfaces. The metal electrodes can be Au, Ag, Pt, Ga, etc., to obtain the required device for high-energy ray detectors.

[0128] Optionally, the resistivity of the high-energy ray detector made of the perovskite single crystal grown in the present application is 5 to 9×10 10 Ω·cm. In some specific embodiments, the resistivity of the high energy ray detector may be 5×10 10 Ω·cm、6×10 10 Ω·cm、7×10 10 Ω·cm、8×10 10 Ω·cm or 9×10 10 Ω·cm. Optionally, the high energy ray detector 137 The energy resolution of the 662keV gamma ray emitted by Cs is 2-3%.137 The energy resolution of the 662 keV gamma ray emitted by Cs can be 2%, 2.2%, 2.4%, 2.6%, 2.8% or 3%.

[0129] The following is a further example of the present invention by taking the preparation process of Cs2AgBiBr6 (CABB for short) as an example:

[0130] First, the first raw material is determined by step S1. The basic elements of CABB include Cs, Ag, Bi and Br, and the first raw material includes CsBr, AgBr and BiBr3. According to the stoichiometric ratio of CABB, raw materials such as CsBr 19.153g, AgBr 8.450g and BiBr3 20.191g can be prepared. Specifically, high-purity (such as ≥5N) CsBr, AgBr and BiBr3 powders can be selected.

[0131] Then, the second raw material is determined by using steps S2-S3, by sorting Cs, Ag, Bi and Br in ascending order according to the probability of forming vacancies in perovskite, selecting the top three Br, Bi and Ag as target elements, and using BiBr3 or AgBr as the second raw material. Specifically, high-purity (such as 7N) BiBr3 powder or AgBr powder can be selected. The second raw material is 2-5wt% of the first raw material, such as 0.95g-2.39g.

[0132] Next, in step S4, a perovskite single crystal is prepared based on the determined first raw material and second raw material.

[0133] First, the first raw material is synthesized into a perovskite polycrystalline material by step S41. The specific process may include: in a dry glove box, the raw materials CsBr 19.153g, AgBr 8.450g, and BiBr3 20.191g are weighed according to the stoichiometric ratio and loaded into a clean third crucible. The cone angle of the third crucible is 47°. The vacuum degree of the third crucible is evacuated to 5×10 -4 Pa, sinter and seal, and put into the second furnace body of the synthesis furnace. The temperature of the second furnace body is first raised to 600℃ over 8 hours and kept warm for 5 hours, so that the CsBr raw material with the highest melting point is fully overheated, the raw materials are fully melted, convected, and evenly mixed to avoid the formation of CsBr inclusion phase; then the temperature is reduced to 470℃ within 1.5 hours and kept warm for 10 to 15 hours to make the raw materials react completely; finally, it is slowly cooled to room temperature to obtain CABB polycrystalline material.

[0134] Then, the CABB polycrystalline material is purified by step S42. The specific process may include: placing the synthesized CABB polycrystalline material into the second crucible of a vertical Bridgman descending furnace having at least two temperature zones for rapid Bridgman descending method purification. The temperature of the first temperature zone is set to 460-480°C, and the temperature of the second temperature zone is set to 250-300°C. The temperature is raised to the target temperature at a rate of 50-70°C / h, and the temperature gradient of the gradient temperature zone can reach 30-50°C / cm. The speed at which the crucible descends from the first temperature zone is 3-20mm / h. After the descent is completed, the second crucible is naturally cooled to room temperature with the furnace to obtain a purified CABB polycrystalline ingot. Take out the purified polycrystalline ingot, remove the tail impurities, and obtain a purified CABB polycrystalline material.

[0135] Finally, step S43 is used to generate a perovskite single crystal from the perovskite polycrystalline material and the second raw material. The specific process may include: replacing the second base in the vertical Bridgman descending furnace with the first base and the metal rod. The seed crystal processed by precise orientation is placed in the first crucible. Then 1.0g of 7N high-purity BiBr3 powder (or 0.95g of AgBr powder raw material) is added above the seed crystal. The powder needs to be ground until there is no agglomeration before being loaded into the first crucible. Finally, the purified CABB polycrystalline material is loaded and vacuumed to 5×10 - 4 Pa and sinter and seal the first crucible. Raise the first temperature zone and the second temperature zone to 480℃ and 390℃ respectively within 3 hours. After the temperature stabilizes, raise the first crucible to a suitable position so that the seed crystal is located in the gradient temperature zone. Keep warm for 6 to 10 hours to fully melt the polycrystalline material and partially melt the seed crystal. Then control the first crucible to slowly descend at a speed of 0.3 to 1 mm / h through the lifting control mechanism until the melt is fully crystallized and the single crystal growth is completed, and then stop descending.

[0136] The temperature of the first and second temperature zones was adjusted to 250-350℃ and kept for 10 hours to perform in-situ annealing on the single crystal. After the annealing was completed, the temperature was slowly lowered to room temperature at a cooling rate of 10-30℃ / h to discharge the thermal stress inside the crystal. After the cooling was completed, the crucible was taken out and the single crystal was obtained. A complete CABB single crystal.

[0137] The CABB crystal was processed into a rough wafer with a thickness of 3 mm. The rough wafer was coarsely and finely ground with sandpaper, and then the wafer surface was polished to obtain a wafer with a smooth surface and a thickness of 1.5 mm. The metal electrodes were evaporated on the upper and lower surfaces of the processed wafer by vacuum thermal evaporation. The metal electrodes can be Au, Ag, Pt, Ga, etc. When Au electrodes were used, the resistivity of the tested CABB device reached 8.4×10 10 Ω·cm, for 137 The energy resolution of the 662keV gamma rays emitted by Cs is 2.9%.

[0138] It can be seen from the above that the technical solution of the present invention can obtain perovskite single crystals with high resistivity, low defect density and large size.

[0139] Obviously, the above embodiments are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the protection scope of the present invention.

Claims

1. A method for preparing a perovskite single crystal, characterized in that: include: Using a raw material prepared according to the basic elements included in the perovskite chemical formula and the stoichiometric ratio between the basic elements as a first raw material; Determining a target element from the basic elements according to the probability of each basic element forming a vacancy in the perovskite; wherein the probability of the target element forming a vacancy in the perovskite is not less than the probability of other elements forming a vacancy in the perovskite; Using a raw material composed of the target element as a second raw material; and A perovskite single crystal is prepared based on the first raw material and the second raw material.

2. The preparation method according to claim 1, characterized in that: The second raw material is 2-5 wt % of the total amount of the first raw material.

3. The preparation method according to claim 1, characterized in that: According to the probability of each basic element forming a vacancy in the perovskite, determining the target element from the basic elements comprises: Sort the basic elements in ascending or descending order according to the probability of forming vacancies in the perovskite, and select the elements in the first N positions in descending order or the last N positions in ascending order from the basic elements as target elements, where N is an integer greater than or equal to 2; Optionally, the target element includes a halogen and at least one monovalent, divalent or trivalent ion; using a raw material composed of the target element as the second raw material comprises: A compound consisting of halogen and other target elements is used as the second raw material.

4. The preparation method according to claim 3, characterized in that: When the chemical formula of the perovskite is ABX3, the target element includes B and X, the second raw material includes BX2; wherein the A ion includes Rb + and / or Cs + , B ions include Sn 2+ and / or Pb 2+ , X ions include Cl – Br – and I – One or more of; or When the chemical formula of the perovskite is A2B Ⅰ B Ⅲ When X6, the target elements include X and B Ⅰ and / or B Ⅲ The second raw material includes B Ⅰ X and / or B Ⅲ X3; where A ions include Rb + and / or Cs + , B Ⅰ Ions include Li + 、Na + , K + , Rb + 、Ag + One or more of B Ⅲ Ions include Al 3+ , Ga 3+ 、In 3+ , Tl 3+ 、Bi 3+ , Sb 3+ One or more of the X ions include Cl – Br – and I – One or more of .

5. The preparation method according to claim 1, characterized in that: Based on the first raw material and the second raw material, preparing a perovskite single crystal includes: synthesizing the first raw material into a perovskite polycrystalline material; Purifying the perovskite polycrystalline material; and The perovskite single crystal is generated by using the perovskite polycrystalline material and the second raw material.

6. The preparation method according to claim 5, characterized in that: Purifying the perovskite polycrystalline material comprises: Keeping the perovskite polycrystalline material warm in a first temperature zone having a first temperature until the perovskite polycrystalline material is melted; Moving the melted perovskite polycrystalline material from the first temperature zone to a second temperature zone having a second temperature; wherein a gradient temperature zone is provided between the first temperature zone and the second temperature zone; and Removing impurities accumulated at the tail end of the perovskite polycrystalline material; Optionally, the first temperature is 20°C to 100°C higher than the melting point of the perovskite single crystal, and the second temperature is 20°C to 100°C lower than the melting point of the perovskite single crystal; Optionally, the temperature gradient of the gradient temperature zone is 30-50° C. / cm.

7. The preparation method according to claim 6, characterized in that: The moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 3 to 20 mm / h, or the moving speed of the melted perovskite polycrystalline material from the first temperature zone to the second temperature zone is 10 to 20 times the descending speed when the perovskite single crystal is grown by the Bridgman method.

8. The preparation method according to claim 5, characterized in that: Generating the perovskite single crystal by using the perovskite polycrystalline material and the second raw material comprises: placing the seed crystal for inducing the growth of the perovskite single crystal, the second raw material and the perovskite polycrystalline material into the first crucible in order from bottom to top; and placing the first crucible into a first furnace body, and growing a perovskite single crystal by a Bridgman method; Optionally, the descending speed when growing the perovskite single crystal by the Bridgman method is 0.3-1 mm / h.

9. The preparation method according to claim 1, characterized in that: Also includes: Annealing the perovskite single crystal; Optionally, the annealing temperature is 250-350° C., and the annealing time is 6-14 h; Optionally, after annealing is completed, the perovskite single crystal is cooled to room temperature at a rate of 10 to 30° C. / h.

10. A system for preparing a perovskite single crystal, characterized in that: include: A first crucible includes a first body for containing a first raw material and a second raw material; wherein the first raw material is a raw material prepared according to the basic elements included in the perovskite chemical formula and the stoichiometric ratio between the basic elements, and the second raw material is a raw material composed of a target element, wherein the target element is a target element determined from the basic elements according to the probability of each basic element forming a vacancy in the perovskite, and the probability of the target element forming a vacancy in the perovskite is not less than the probability of other elements forming a vacancy in the perovskite; and The first furnace body is used to accommodate the first crucible and provide a required temperature environment for preparing a perovskite single crystal based on the first raw material and the second raw material.

11. The preparation system according to claim 10, characterized in that: The first furnace body comprises a furnace cavity for accommodating the first crucible; A first bottom support for supporting the first crucible is arranged in the furnace chamber, and the first bottom support and the first crucible are connected via a metal rod with heat conduction function; Optionally, a water-cooling rod that penetrates the furnace cavity and can move up and down in the furnace cavity is connected to the bottom of the first base, and a lifting control mechanism is connected to the bottom of the water-cooling rod to control the water-cooling rod to drive the first crucible to move in the furnace cavity.

12. The preparation system according to claim 11, characterized in that: The metal rod is made of one or more of silver, aluminum, copper and zinc.

13. The preparation system according to claim 11, characterized in that: A first heating element, a second heating element and a heat insulation plate between the first heating element and the second heating element are arranged on the side wall of the furnace cavity; wherein the first heating element can form a first temperature zone in the first furnace body after being heated, the second heating element can form a second temperature zone in the first furnace body after being heated, and the heat insulation board can form a gradient temperature zone in the first furnace body after the first heating element and the second heating element are heated; Optionally, the height of the first temperature zone is 250-350 mm, the height of the gradient temperature zone is 20-30 mm, and the height of the second temperature zone is 150-250 mm.

14. A perovskite single crystal, characterized in that: The method is obtained by the preparation method described in any one of claims 1 to 9 or the preparation system described in any one of claims 10 to 13.

15. A high energy ray detector, characterized in that: The perovskite single crystal according to claim 14; Optionally, the resistivity of the high energy ray detector is 5 to 9×10 10 Ω·cm; Optionally, the high energy ray detector is 137 The energy resolution of the 662keV gamma rays emitted by Cs is 2-3%.