A method for preparing high electron mobility IGTO doped target material

By using gallium oxide, tin oxide, silicon-doped iron oxide and indium oxide powder to prepare high electron mobility IGTO-doped targets, the contradiction between mobility and stability in amorphous indium oxide-based TFT is solved, and the Thin film transistors with high switching current ratio, mobility and excellent bias stability improve device performance and reliability.

CN118894720BActive Publication Date: 2024-12-03WUHU YINGRI TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411400884.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-03
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

In the industrialization process, amorphous indium oxide-based TFTs face mutual constraints between mobility and stability, resulting in unstable device characteristics.

Method used

Using gallium oxide, tin oxide, silicon-doped iron oxide and indium oxide powder as raw materials, high electron mobility IGTO-doped targets are prepared through spray granulation and high-pressure sintering processes to improve relative density and resistivity and reduce bias threshold Voltage change to enhance device stability.

Benefits of technology

Thin film transistors with high switching current ratio and high mobility have excellent bias voltage stability, overcome the problem of stability reduction caused by the addition of iron oxide, and improve the reliability and energy utilization efficiency of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894720B_ABST
    Figure CN118894720B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of target material technology, and in particular to a method for preparing an IGTO-doped target material with high electron mobility. The preparation method comprises the following steps: firstly ball-milling oxide powder to obtain a mixed slurry, then granulating the mixed slurry, and finally obtaining an IGTO-doped target material with high electron mobility by molding and sintering; the oxide powder comprises by weight percentage: 1.5%-3% gallium oxide powder, 0.7%-1.2% tin oxide powder, 0.4%-0.6% silicon-doped iron oxide powder and the remainder of indium oxide powder. The IGTO-doped target material prepared by the present invention has high relative density and low resistivity, and the thin film transistor prepared by the IGTO-doped target material has high mobility and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target materials, and in particular to a method for preparing an IGTO doped target material with high electron mobility. Background Art

[0002] Thin-film transistors (TFTs) are an indispensable part of the modern display field (as the switch and driving unit of the pixel). TFT is one of the oldest electronic devices and a type of field-effect transistor (FET) with a history of more than 80 years. Its preparation method is to deposit different thin films on the substrate, such as electrodes, insulating layers, active layers, etc. The order of thin film deposition is different in TFTs of different structures. The material type and preparation process of the active layer have a key influence on the performance of the device.

[0003] As active layer materials in TFTs, amorphous indium oxide-based materials have the advantages of high field effect mobility, low preparation temperature, flexibility and transparency, and are widely used in the display field. These advantages make it an important choice for pursuing high-resolution and high-refresh rate display technologies. However, there is a mutually restrictive relationship between the mobility and stability of amorphous indium oxide-based TFTs, which leads to challenges in its industrialization process.

[0004] As an active layer material, gallium-doped indium tin oxide (IGTO) target can effectively enhance mobility and have a higher carrier concentration, thereby improving its performance. However, this also leads to instability in device characteristics. Therefore, optimizing the performance of IGTO TFT requires focusing on improving mobility while ensuring stability. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a method for preparing a high electron mobility IGTO doped target material so as to improve the mobility of amorphous indium oxide-based TFTs without significantly reducing the stability.

[0006] Based on the above purpose, the present invention provides a method for preparing a high electron mobility IGTO doped target, comprising the following steps: first ball milling oxide powder to obtain a mixed slurry, then spray granulating the mixed slurry to obtain a mixed powder, and finally obtaining a high electron mobility IGTO doped target by molding and sintering.

[0007] Furthermore, the oxide powder comprises, by weight percentage: 1.5%-3% gallium oxide powder, 0.7%-1.2% tin oxide powder, 0.4%-0.6% silicon-doped iron oxide powder and the balance indium oxide powder.

[0008] Furthermore, the preparation method of the silicon-doped iron oxide powder is as follows: adding ferric nitrate nonahydrate to deionized water, stirring to dissolve, then using nitric acid solution to adjust the pH to 2-3, then adding sodium silicate solution dropwise, after the addition is complete, using sodium hydroxide solution to adjust the pH to 12-13, standing at room temperature for 60 minutes, then heating to 70°C, standing for 12 hours, purifying, drying, and then calcining at 360-380°C for 2.5-3.5 hours in an oxygen atmosphere, ball milling, and obtaining a specific surface area of ​​5-8m 2 / g of silicon-doped iron oxide powder.

[0009] Furthermore, the molar ratio of the ferric nitrate nonahydrate to sodium silicate is 1:0.2-0.4.

[0010] Preferably, the concentration of the nitric acid solution is 0.1 mol / L, and the concentration of the sodium hydroxide solution is 0.1 mol / L.

[0011] Preferably, the concentration of the sodium silicate solution is 1 mol / L.

[0012] Preferably, the specific surface area of ​​the indium oxide powder is 5-10 m 2 / g, the specific surface area of ​​gallium oxide powder is 4-8m 2 / g, the specific surface area of ​​tin oxide powder is 6-10m 2 / g.

[0013] Preferably, the particle size distribution D50 of the mixed slurry is 0.3-0.4 μm.

[0014] Preferably, the particle size D50 of the mixed powder is 30-35 μm, and the bulk density is 1.5-1.7 g / cm 3 .

[0015] Preferably, the molding pressure is 280-320 MPa, and the molding time is 35-45 min.

[0016] Preferably, the sintering adopts gradient temperature rising sintering, and the specific procedure is: in air atmosphere, under normal pressure, the temperature is raised from room temperature to 300°C at 2-3°C / min, and kept warm for 0.4-0.6h; then in oxygen atmosphere, under pressure of 0.5MPa, the temperature is raised from 300°C to 600°C at 2-3°C / min, and kept warm for 3-5h; then in oxygen atmosphere, under pressure of 0.5MPa, the temperature is raised from 600°C to 1200°C at 5-7°C / min, and kept warm for 14-16h; then in oxygen atmosphere, under pressure of 1MPa, the temperature is raised from 1200°C to 1500°C at 0.5-2°C / min, and kept warm for 8-12h; finally in oxygen atmosphere, under pressure of 0.5MPa, the temperature is lowered to room temperature at 15-20°C / min.

[0017] Beneficial effects of the present invention:

[0018] The present invention uses silicon-doped iron oxide powder, indium oxide powder, gallium oxide powder and tin oxide powder as raw materials to synthesize IGTO doped target materials. The silicon-doped iron oxide powder improves the relative density and resistivity of the IGTO doped target materials. The thin film transistor prepared by using the silicon-doped iron oxide powder has a high switching current ratio and a high mobility. Moreover, after a -20 V bias voltage is applied for 3600 s, ΔV th As low as -0.66V, with excellent bias stability.

[0019] The silicon doping of iron oxide in the present invention helps to maintain the switching current ratio and mobility of the thin film transistor while reducing the change in bias threshold voltage, thus overcoming the problem of decreased stability caused by the addition of iron oxide.

[0020] The present invention adopts high-pressure sintering, which helps to suppress oxygen vacancies in the thin film transistor, effectively avoiding the influence of extra electrons provided by the oxygen vacancies on the threshold voltage, thereby reducing the change in bias threshold voltage and improving stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required to be used in the embodiments or the description of the prior art are briefly introduced below.

[0022] Figure 1 This is a cross-sectional picture of the high electron mobility IGTO doped target material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0024] Embodiment 1:

[0025] (1) Add 4.04 g of ferric nitrate nonahydrate to 100 mL of deionized water, stir to dissolve, then use 0.1 mol / L nitric acid solution to adjust the pH to 2.4, then add 3 ml of 1 mol / L sodium silicate solution, after the addition is complete, use 0.1 mol / L sodium hydroxide solution to adjust the pH to 12.6, let stand at room temperature for 60 min, then heat to 70 °C, let stand for 12 h, filter, wash with deionized water 3 times, dry at 80 °C for 12 h, then calcine at 375 °C for 3 h in an oxygen atmosphere, and ball mill to obtain a specific surface area of ​​6.5 m 2 / g of silicon-doped iron oxide powder;

[0026] (2) 96.5g of a specific surface area of ​​7.5m 2 / g indium oxide powder, 2g specific surface area is 6.2m2 / g of gallium oxide powder, with a specific surface area of ​​8.3m 2 / g of tin oxide powder and 0.5g of specific surface area of ​​6.5m 2 / g silicon-doped iron oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.35μm;

[0027] (3) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 32 μm and the bulk density = 1.6 g / cm 3 Mixed powder;

[0028] (4) The mixed powder is loaded into a mold for molding, the molding pressure is set to 300 MPa, and the molding time is set to 40 min to obtain a green blank;

[0029] (5) The green blank is placed in a sintering furnace for sintering, and a gradient temperature rise sintering is adopted. In an air atmosphere, at normal pressure, the temperature is raised from room temperature to 300°C at a rate of 2.5°C / min, and the temperature is kept at this temperature for 0.5 h. Then, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 2.5°C / min, and the temperature is kept at this temperature for 4 h. Then, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 6°C / min, and the temperature is kept at this temperature for 15 h. Then, in an oxygen atmosphere, at a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 1°C / min, and the temperature is kept at this temperature for 10 h. Finally, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 20°C / min, and a high electron mobility IGTO doped target is obtained.

[0030] Embodiment 2:

[0031] (1) Add 4.04 g of ferric nitrate nonahydrate to 100 mL of deionized water, stir to dissolve, then use 0.1 mol / L nitric acid solution to adjust the pH to 2.1, then add 2 ml of 1 mol / L sodium silicate solution, after the addition is complete, use 0.1 mol / L sodium hydroxide solution to adjust the pH to 12, let stand at room temperature for 60 min, then heat to 70 °C, let stand for 12 h, filter, wash with deionized water 3 times, dry at 80 °C for 12 h, then calcine at 360 °C for 3.5 h in an oxygen atmosphere, and ball mill to obtain a specific surface area of ​​5.2 m 2 / g of silicon-doped iron oxide powder;

[0032] (2) 97.4g of a specific surface area of ​​7.5m 2 / g indium oxide powder, 1.5g specific surface area is 6.2m 2 / g of gallium oxide powder, 0.7g specific surface area of ​​8.3m2 / g of tin oxide powder and 0.4g of specific surface area of ​​5.2m 2 / g silicon-doped iron oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.32μm;

[0033] (3) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 31 μm and the bulk density = 1.5 g / cm 3 Mixed powder;

[0034] (4) The mixed powder is placed in a mold for molding, the molding pressure is set to 280 MPa, and the molding time is set to 45 min to obtain a green blank;

[0035] (5) The green blank is placed in a sintering furnace for sintering, and a gradient temperature rise sintering is adopted. In an air atmosphere, at normal pressure, the temperature is raised from room temperature to 300°C at a rate of 2°C / min, and the temperature is kept at this temperature for 0.4 h. Then, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 2°C / min, and the temperature is kept at this temperature for 3 h. Then, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 5°C / min, and the temperature is kept at this temperature for 14 h. Then, in an oxygen atmosphere, at a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 0.5°C / min, and the temperature is kept at this temperature for 8 h. Finally, in an oxygen atmosphere, at a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 15°C / min, and a high electron mobility IGTO doped target is obtained.

[0036] Embodiment 3:

[0037] (1) Add 4.04 g of ferric nitrate nonahydrate to 100 mL of deionized water, stir to dissolve, then use 0.1 mol / L nitric acid solution to adjust the pH to 2.8, then add 4 ml of 1 mol / L sodium silicate solution, after the addition is complete, use 0.1 mol / L sodium hydroxide solution to adjust the pH to 12.9, let stand at room temperature for 60 min, then heat to 70 °C, let stand for 12 h, filter, wash with deionized water 3 times, dry at 80 °C for 12 h, then calcine at 380 °C for 2.5 h in an oxygen atmosphere, and ball mill to obtain a specific surface area of ​​7.8 m 2 / g of silicon-doped iron oxide powder;

[0038] (2) 95.2g of a specific surface area of ​​7.5m 2 / g indium oxide powder, 3g specific surface area is 6.2m 2 / g of gallium oxide powder, 1.2g of specific surface area is 8.3m 2 / g of tin oxide powder and 0.6g of specific surface area of ​​7.8m2 / g silicon-doped iron oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size D50 = 0.38μm;

[0039] (3) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 34 μm and the bulk density = 1.7 g / cm 3 Mixed powder;

[0040] (4) The mixed powder is placed in a mold for molding, the molding pressure is set to 320 MPa, and the molding time is set to 35 min to obtain a green blank;

[0041] (5) The green blank is placed in a sintering furnace and sintered using a gradient temperature rise sintering method. In an air atmosphere and normal pressure, the temperature is raised from room temperature to 300°C at a rate of 3°C / min and kept at this temperature for 0.6 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 3°C / min and kept at this temperature for 5 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 7°C / min and kept at this temperature for 16 h. Then, in an oxygen atmosphere and a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 2°C / min and kept at this temperature for 12 h. Finally, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 20°C / min to obtain a high electron mobility IGTO doped target.

[0042] Comparative Example 1:

[0043] The difference between Comparative Example 1 and Example 1 is that: silicon-doped iron oxide powder is not added in step (2);

[0044] The specific steps are as follows:

[0045] (1) 96.5 g of a specific surface area of ​​7.5 m 2 / g indium oxide powder, 2g specific surface area is 6.2m 2 / g of gallium oxide powder, with a specific surface area of ​​8.3m 2 / g of tin oxide powder was added into a ball mill, and then 100g of deionized water and 1g of polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.36μm;

[0046] (2) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 33 μm and the bulk density = 1.5 g / cm 3 Mixed powder;

[0047] (3) The mixed powder is placed in a mold for molding, the molding pressure is set to 300 MPa, and the molding time is set to 40 min to obtain a green blank;

[0048] (4) Place the green blank in a sintering furnace and sinter it using a gradient temperature rise sintering method. In an air atmosphere and normal pressure, the temperature is raised from room temperature to 300°C at a rate of 2.5°C / min, and the temperature is kept for 0.5 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 2.5°C / min, and the temperature is kept for 4 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 6°C / min, and the temperature is kept for 15 h. Then, in an oxygen atmosphere and a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 1°C / min, and the temperature is kept for 10 h. Finally, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 20°C / min to obtain a target material.

[0049] Comparative Example 2:

[0050] The difference between Comparative Example 2 and Example 1 is that: the specific surface area of ​​6.5 m 2 / g of silicon-doped iron oxide powder was replaced with a specific surface area of ​​6.4m 2 / g iron oxide powder;

[0051] The specific steps are as follows:

[0052] (2) 96.5g of a specific surface area of ​​7.5m 2 / g indium oxide powder, 2g specific surface area is 6.2m 2 / g of gallium oxide powder, with a specific surface area of ​​8.3m 2 / g of tin oxide powder and 0.5g of specific surface area of ​​6.4m 2 / g iron oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.34μm;

[0053] (3) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 33 μm and the bulk density = 1.6 g / cm 3 Mixed powder;

[0054] (4) The mixed powder is loaded into a mold for molding, the molding pressure is set to 300 MPa, and the molding time is set to 40 min to obtain a green blank;

[0055] (5) Place the green blank in a sintering furnace and sinter it using a gradient temperature rise sintering method. In an air atmosphere and normal pressure, the temperature is raised from room temperature to 300°C at a rate of 2.5°C / min, and the temperature is kept for 0.5 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 2.5°C / min, and the temperature is kept for 4 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 6°C / min, and the temperature is kept for 15 h. Then, in an oxygen atmosphere and a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 1°C / min, and the temperature is kept for 10 h. Finally, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 20°C / min to obtain a target material.

[0056] Comparative Example 3:

[0057] The difference between Comparative Example 3 and Example 1 is that the specific surface area of ​​6.5 m 2 / g of silicon-doped iron oxide powder was replaced with a specific surface area of ​​6.4m 2 / g iron oxide powder and a specific surface area of ​​6.6m 2 / g of silicon oxide powder in a weight ratio of 4:1;

[0058] The specific steps are as follows:

[0059] (1) 96.5 g of a specific surface area of ​​7.5 m 2 / g indium oxide powder, 2g specific surface area is 6.2m 2 / g of gallium oxide powder, with a specific surface area of ​​8.3m 2 / g of tin oxide powder, 4g of specific surface area is 6.4m 2 / g iron oxide powder and 1g specific surface area is 6.6m 2 / g silicon oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.36μm;

[0060] (2) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 34 μm and the bulk density = 1.8 g / cm 3 Mixed powder;

[0061] (3) The mixed powder is placed in a mold for molding, the molding pressure is set to 300 MPa, and the molding time is set to 40 min to obtain a green blank;

[0062] (4) Place the green blank in a sintering furnace and sinter it using a gradient temperature rise sintering method. In an air atmosphere and normal pressure, the temperature is raised from room temperature to 300°C at a rate of 2.5°C / min, and the temperature is kept for 0.5 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 300°C to 600°C at a rate of 2.5°C / min, and the temperature is kept for 4 h. Then, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is raised from 600°C to 1200°C at a rate of 6°C / min, and the temperature is kept for 15 h. Then, in an oxygen atmosphere and a pressure of 1 MPa, the temperature is raised from 1200°C to 1500°C at a rate of 1°C / min, and the temperature is kept for 10 h. Finally, in an oxygen atmosphere and a pressure of 0.5 MPa, the temperature is lowered to room temperature at a rate of 20°C / min to obtain a target material.

[0063] Comparative Example 4:

[0064] The difference between Comparative Example 4 and Example 1 is that: the sintering in step (5) is carried out under normal pressure;

[0065] The specific steps are as follows:

[0066] (1) Add 4.04 g of ferric nitrate nonahydrate to 100 mL of deionized water, stir to dissolve, then use 0.1 mol / L nitric acid solution to adjust the pH to 2.4, then add 3 ml of 1 mol / L sodium silicate solution, after the addition is complete, use 0.1 mol / L sodium hydroxide solution to adjust the pH to 12.6, let stand at room temperature for 60 min, then heat to 70 °C, let stand for 12 h, filter, wash with deionized water 3 times, dry at 80 °C for 12 h, then calcine at 375 °C for 3 h in an oxygen atmosphere, and ball mill to obtain a specific surface area of ​​6.5 m 2 / g of silicon-doped iron oxide powder;

[0067] (2) 96.5g of a specific surface area of ​​7.5m 2 / g indium oxide powder, 2g specific surface area is 6.2m 2 / g of gallium oxide powder, with a specific surface area of ​​8.3m 2 / g of tin oxide powder and 0.5g of specific surface area of ​​6.5m 2 / g silicon-doped iron oxide powder was added into a ball mill, and then 100g deionized water and 1g polyvinyl alcohol 1788 were added, and ball milling was performed to obtain a mixed slurry with a particle size of D50 = 0.354μm;

[0068] (3) The mixed slurry was placed in a centrifugal spray granulator for drying and granulation. The inlet air temperature was set to 220°C and the outlet air temperature was set to 100°C. The powder particle size D50 = 32 μm and the bulk density = 1.6 g / cm 3 Mixed powder;

[0069] (4) The mixed powder is loaded into a mold for molding, the molding pressure is set to 300 MPa, and the molding time is set to 40 min to obtain a green blank;

[0070] (5) Place the green blank in a sintering furnace and sinter it using a gradient temperature rise sintering method: in an air atmosphere and normal pressure, heat it from room temperature to 300°C at a rate of 2.5°C / min, and keep it at that temperature for 0.5 h. Then, in an oxygen atmosphere and normal pressure, heat it from 300°C to 600°C at a rate of 2.5°C / min, and keep it at that temperature for 4 h. Then, in an oxygen atmosphere and normal pressure, heat it from 600°C to 1200°C at a rate of 6°C / min, and keep it at that temperature for 15 h. Then, in an oxygen atmosphere and normal pressure, heat it from 1200°C to 1500°C at a rate of 1°C / min, and keep it at that temperature for 10 h. Finally, in an oxygen atmosphere and normal pressure, cool it to room temperature at a rate of 20°C / min to obtain a target material.

[0071] Target performance test:

[0072] The relative density of the target materials prepared in the embodiment and the comparative example was tested by the Archimedes drainage method, and the resistivity was tested by a resistivity tester. The results are shown in Table 1.

[0073] Table 1 Target properties

[0074] sample Relative density Resistivity / μΩ·m Example 1 99.91 235 Example 2 99.86 221 Example 3 99.89 239 Comparative Example 1 98.25 456 Comparative Example 2 99.75 211 Comparative Example 3 99.18 1358 Comparative Example 4 99.12 269

[0075] Data Analysis:

[0076] It can be seen from the data of Examples 1-3 in Table 1 that the IGTO-doped target material prepared by the present invention has a high relative density and a low resistivity. A target material with a high relative density usually means fewer pores and defects, which helps to improve the uniformity and stability of the material during the sputtering process, and further promotes the formation of a dense and uniform film. The target material with a low resistivity can effectively improve the conductive properties of the film. The low resistivity ensures the high conductivity of the film in the electronic device, reduces the energy loss during the electron transmission process, and thus improves the efficiency and performance of the device.

[0077] It can be seen from the data of Example 1 and Comparative Example 1 in Table 1 that silicon-doped iron oxide powder helps to further reduce the resistivity of the IGTO-doped target.

[0078] It can be seen from the data of Example 1 and Comparative Example 2 in Table 1 that the doping of silicon in the iron oxide powder has little effect on the relative density and resistivity of the target material.

[0079] It can be seen from the data of Example 1 and Comparative Example 3 in Table 1 that the mixed doping of iron oxide powder and silicon oxide powder will lead to a significant decrease in the relative density of the IGTO doped target and a significant increase in the resistivity.

[0080] It can be seen from the data of Example 1 and Comparative Example 4 in Table 1 that, compared with sintering under normal pressure, high pressure sintering helps to increase the relative density.

[0081] Preparation of thin film transistor: The thin film transistor includes a substrate, an IGTO active layer, a source electrode and a drain electrode from bottom to top, the source electrode and the drain electrode are grown on the IGTO active layer, the substrate is a P-Si with 100 nm thick SiO2 grown by surface thermal oxidation, the source electrode and the drain electrode are both made of Au, the IGTO active layer is obtained by radio frequency magnetron sputtering of the target material prepared in the embodiment and the comparative example, the sputtering power of the radio frequency magnetron sputtering is 90W, the sputtering time is 15min, and the sputtering is annealed at 230°C for 1h after the sputtering.

[0082] Thin film transistor performance test:

[0083] Basic electrical performance: Tested using a semiconductor parameter analyzer, setting the drain voltage V DS is 10.1V, the gate voltage V G The switching current ratio I of the thin film transistors corresponding to the embodiment and the comparative example is obtained from -15V to +15V with an interval of 0.5V. on / I off and saturation mobility μ sat , the results are shown in Table 2.

[0084] Bias stability: Tested using a semiconductor parameter analyzer, setting the drain voltage V DS is 10.1V, the gate voltage V G -15V to +15V, with an interval of 0.5V, and a gate bias voltage V Gstress The change in negative bias threshold voltage ∆V is obtained when the voltage is -20V and the time is 600-3600s. th The smaller the change in bias threshold voltage, the better the stability of the transfer curve under long-term bias. The results are shown in Table 2.

[0085] Table 2 Thin film transistor performance

[0086]

[0087] Data Analysis:

[0088] From the data of Examples 1-3 in Table 2, it can be seen that the thin film transistor prepared by using the high electron mobility IGTO doped target provided by the present invention has a high switching current ratio and high mobility. The high switching current ratio means faster switching speed and higher signal processing capability, and the high mobility increases the carrier mobility, enhances the current driving capability, reduces power consumption, and improves the overall efficiency of the device. The combination of these two enables TFT to have better response speed and higher energy utilization efficiency in displays and other electronic devices. Most importantly, after -20 V bias is applied for 3600 s, ΔV th As low as -0.66V, it shows that its transfer curve does not shift seriously under long-term bias, and has excellent bias stability. The excellent bias stability improves the reliability of the device, ensures that it can still work normally under high voltage conditions, and reduces performance degradation.

[0089] It can be seen from the data of Example 1 and Comparative Example 1 in Table 2 that the silicon-doped iron oxide powder effectively improves the switching current ratio and mobility of the thin film transistor and reduces the change in bias threshold voltage.

[0090] It can be seen from the data of Example 1 and Comparative Examples 1-3 in Table 2 that the addition of iron oxide powder can effectively improve the switching current ratio and mobility of the thin film transistor, but greatly increase the change in bias threshold voltage and reduce the stability. Silicon doping helps to maintain the switching current ratio and mobility of the thin film transistor while reducing the change in bias threshold voltage, overcoming the problem of decreased stability caused by the addition of iron oxide. This may be because silicon suppresses oxygen vacancies in the thin film transistor, effectively avoiding the influence of additional electrons provided by oxygen vacancies on the threshold voltage.

[0091] It can be seen from the data of Example 2 and Comparative Example 4 that, compared with sintering at normal pressure, high pressure sintering helps to reduce the change in bias threshold voltage, improve stability, and has little effect on the switching current ratio and mobility.

[0092] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A method for preparing a high electron mobility IGTO doped target material, It is characterized in that The method comprises the following steps: firstly ball-milling oxide powder to obtain a mixed slurry, then spray-granulating the mixed slurry to obtain a mixed powder, and finally obtaining a high electron mobility IGTO doped target material by molding and sintering; The oxide powder comprises, by weight percentage: 1.5%-3% gallium oxide powder, 0.7%-1.2% tin oxide powder, 0.4%-0.6% silicon-doped iron oxide powder and the balance indium oxide powder; The preparation method of the silicon-doped iron oxide powder is as follows: Add ferric nitrate nonahydrate into deionized water, stir and dissolve, then use nitric acid solution to adjust the pH to 2-3, then add sodium silicate solution dropwise, after the addition is complete, use sodium hydroxide solution to adjust the pH to 12-13, let stand at room temperature for 60 minutes, then heat to 70°C, let stand for 12 hours, purify, dry, then calcine at 360-380°C for 2.5-3.5 hours in an oxygen atmosphere, and ball mill to obtain a specific surface area of ​​5-8m 2 / g of silicon-doped iron oxide powder; The molar ratio of the ferric nitrate nonahydrate to the sodium silicate is 1:0.2-0.

4.

2. The method for preparing the high electron mobility IGTO doped target according to claim 1, It is characterized in that The specific surface area of ​​the indium oxide powder is 5-10m 2 / g, the specific surface area of ​​gallium oxide powder is 4-8m 2 / g, the specific surface area of ​​tin oxide powder is 6-10m 2 / g.

3. The method for preparing the high electron mobility IGTO doped target according to claim 1, It is characterized in that The particle size distribution D50 of the mixed slurry is 0.3-0.4 μm.

4. The method for preparing a high electron mobility IGTO doped target according to claim 1, It is characterized in that The particle size D50 of the mixed powder is 30-35 μm, and the bulk density is 1.5-1.7 g / cm 3 .

5. The method for preparing the high electron mobility IGTO doped target according to claim 1, It is characterized in that The molding pressure is 280-320 MPa, and the molding time is 35-45 min.

6. The method for preparing the high electron mobility IGTO doped target according to claim 1, It is characterized in that The sintering adopts gradient temperature rising sintering, and the specific procedure is: in air atmosphere, under normal pressure, the temperature is raised from room temperature to 300°C at 2-3°C / min, and kept warm for 0.4-0.6h; then in oxygen atmosphere, under pressure of 0.5MPa, the temperature is raised from 300°C to 600°C at 2-3°C / min, and kept warm for 3-5h; then in oxygen atmosphere, under pressure of 0.5MPa, the temperature is raised from 600°C to 1200°C at 5-7°C / min, and kept warm for 14-16h; then in oxygen atmosphere, under pressure of 1MPa, the temperature is raised from 1200°C to 1500°C at 0.5-2°C / min, and kept warm for 8-12h; finally in oxygen atmosphere, under pressure of 0.5MPa, the temperature is lowered to room temperature at 15-20°C / min.

7. The method for preparing a high electron mobility IGTO doped target according to claim 1, It is characterized in that The concentration of the nitric acid solution is 0.1 mol / L, and the concentration of the sodium hydroxide solution is 0.1 mol / L.

8. The method for preparing the high electron mobility IGTO doped target according to claim 1, It is characterized in that The concentration of the sodium silicate solution is 1 mol / L.

Citation Information

Patent Citations

  • BiFeO3 target and film production method