Birefringent crystal and preparation method thereof

By preparing SbTeO3F birefringent crystals, the problems of high preparation cost and low light transmittance of birefringent crystal materials in the prior art are solved, and optical materials with high birefringence and stability are realized, which are suitable for optical applications.

CN119061474AActive Publication Date: 2024-12-03SICHUAN NORMAL UNIV

Patent Information

Application Number
CN202411193789.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing birefringent crystal materials have high preparation costs, low light transmittance and low birefringence, which limit their application.

Method used

Using SbTeO3F as the birefringent crystal, a precursor solution is formed by stirring the antimony-containing compound and tellurium-containing compound in a mixed solution. After filtering and standing, the crystals are collected to prepare birefringent crystals with a large birefringent index and good stability. .

Benefits of technology

It has achieved simplification and cost reduction in the preparation process of birefringent crystals, while improving the birefringent index and physical and chemical stability, and is suitable for optical materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061474A_ABST
    Figure CN119061474A_ABST
Patent Text Reader

Abstract

The invention discloses a birefringent crystal and a preparation method thereof, and belongs to the technical field of optical materials. The chemical formula of the birefringent crystal is SbTeO3F; the space group of the birefringent crystal is P212121; and the cell parameters are as follows: # imgabs0 # alpha = 90 degrees, beta = 90 degrees, gamma = 90 degrees, and Z = 4. The preparation method comprises the following steps: dissolving an antimony-containing compound and a tellurium-containing compound in a mixed solution, filtering, and standing filtrate at room temperature for 4-5 days; and then collecting the precipitated crystals, and cleaning to obtain the product. The birefringent crystal disclosed by the invention is simple in preparation process and good in repeatability, and the yield can be improved while the preparation cost is reduced; the obtained birefringent crystal has large birefringence, can be kept stable in air and water, and has good physical and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical materials, and in particular relates to a birefringent crystal and a preparation method thereof. Background Art

[0002] When a beam of light is irradiated onto the surface of a crystal, two beams of refracted light are generated. This phenomenon is called birefringence, and a crystal that can produce birefringence is called a birefringent crystal. The birefringence property of a crystal is an important optical performance parameter of a photoelectric functional material crystal. The characteristics of a birefringent crystal can be used to modulate and detect the polarization state of light, obtain linearly polarized light, and achieve the displacement of a light beam. Therefore, birefringent crystal materials are widely used in the manufacture of key parts of optical isolators, optical modulators, polarization beam splitters, polarizer prisms, and other components.

[0003] The birefringent crystals currently used in commercial applications mainly include TiO 2 (Δn=0.256@546nm), CaCO 3 (Δn=0.172@532nm), YVO 4 (Δn=0.204@53nm), LiNbO 3 (Δn=0.074@546nm) and α-BaB 2 O 4 (Δn=0.122@546nm). The natural birefringent crystal TiO 2 and CaCO 3 Its application is limited due to quality problems such as impurities and defects. 3 、YVO 4 and LiNbO 3 The synthesis of birefringent crystals is relatively expensive, and some birefringent crystals have problems such as low transmittance and small birefringence. Therefore, it is of great significance to find birefringent crystal materials with excellent performance. Summary of the invention

[0004] In view of the above-mentioned prior art, the present invention provides a birefringent crystal and a preparation method thereof to solve the technical problems in the prior art such as high preparation cost of birefringent materials, low light transmittance and small birefringence.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a birefringent crystal, the chemical formula of the birefringent crystal is SbTeO 3 F; the space group of the birefringent crystal is P2 1 2 1 2 1 ; The unit cell parameters are α=90°, β=90°, γ=90°, Z=4.

[0006] The present invention also provides a method for preparing the above-mentioned birefringent crystal, comprising the following steps:

[0007] S1: mixing an antimony-containing compound and a tellurium-containing compound, dissolving the mixture in a mixed solution, and stirring at a stirring rate of 800 to 1200 rpm for 15 to 25 minutes to obtain a precursor solution; the mixed solution is obtained by mixing hydrofluoric acid and distilled water;

[0008] S2: filtering the precursor solution, and allowing the obtained filtrate to stand at room temperature for 4 to 5 days;

[0009] S3: Collect the precipitated crystals and wash them to obtain the product.

[0010] Based on the above technical solution, the present invention can also be improved as follows.

[0011] Furthermore, the antimony-containing compound is SbF 3 , tellurium-containing compounds are TeO 2 .

[0012] Further, SbF 3 and TeO 2 The molar ratio is 4:1.

[0013] Furthermore, the material-liquid ratio of the mixture to the mixed solution is 1 g: 3 to 5 mL.

[0014] Furthermore, the mixed solution is prepared by mixing hydrofluoric acid and distilled water in a volume ratio of 1:25 to 35.

[0015] Further, the mixed solution is prepared by mixing hydrofluoric acid and distilled water in a volume ratio of 1:30.

[0016] Furthermore, in S1, the stirring rate is 1000 rpm and the stirring time is 20 min.

[0017] Furthermore, the cleaning method in S3 is to rinse with distilled water and ethanol 1 to 3 times respectively.

[0018] The beneficial effects of the present invention are:

[0019] 1. The birefringent crystal preparation process of the present invention is simple and has good repeatability, which can reduce the preparation cost and improve the yield.

[0020] 2. The present invention combines two cations ([SbO 3 F] 4- and [TeO 3 ] 3- ) are combined together to form a birefringent crystal with a special unit cell structure. The resulting birefringent crystal has a large birefringence and can remain stable in both air and water, with good physical and chemical stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The formation mechanism diagram of the birefringent crystal SbTeO3F; (a) is [SbO 3 F] 4- and [TeO 3 ] 3- The ball-and-stick coordination mode of SbTeO 3 The three-dimensional framework structure of F;

[0022] Figure 2 is the X-ray powder diffraction pattern of birefringent crystal SbTeO3F;

[0023] Figure 3 For birefringent crystal SbTeO 3 Thermogravimetric spectrum of F;

[0024] Figure 4 For birefringent crystal SbTeO 3 Infrared spectrum of F;

[0025] Figure 5 For birefringent crystal SbTeO 3 UV-visible diffuse reflectance spectrum of F;

[0026] Figure 6 For birefringent crystal SbTeO 3 F birefringence test chart. DETAILED DESCRIPTION

[0027] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0028] Example 1

[0029] A birefringent crystal, the chemical formula of which is SbTeO 3 F; which is prepared by the following steps:

[0030] S1: SbF 3 and TeO 2 The mixture was mixed at a molar ratio of 4:1, and then the mixture was dissolved in the mixed solution at a solid-liquid ratio of 1 g:4 mL, and then stirred at a stirring rate of 1000 rpm for 20 minutes to obtain a precursor solution; the mixed solution was prepared by mixing hydrofluoric acid and distilled water at a volume ratio of 1:30;

[0031] S2: Filter the precursor solution with filter paper, and let the filtrate stand at room temperature for 5 days;

[0032] S3: Collect the precipitated crystals, and rinse them with distilled water and ethanol twice each.

[0033] Example 2

[0034] A birefringent crystal, the chemical formula of which is SbTeO 3 F; which is prepared by the following steps:

[0035] S1: SbF 3 and TeO 2 The mixture was mixed at a molar ratio of 4:1, and then the mixture was dissolved in the mixed solution at a solid-liquid ratio of 1 g:3 mL, and then stirred at a stirring rate of 800 rpm for 25 minutes to obtain a precursor solution; the mixed solution was prepared by mixing hydrofluoric acid and distilled water at a volume ratio of 1:35;

[0036] S2: Filter the precursor solution with filter paper, and let the filtrate stand at room temperature for 4 days;

[0037] S3: Collect the precipitated crystals, and rinse them with distilled water and ethanol respectively once in sequence to obtain the product.

[0038] Example 3

[0039] A birefringent crystal, the chemical formula of which is SbTeO 3 F; which is prepared by the following steps:

[0040] S1: SbF 3 and TeO 2 The mixture was mixed at a molar ratio of 4:1, and then the mixture was dissolved in the mixed solution at a solid-liquid ratio of 1 g:5 mL, and then stirred at a stirring rate of 1200 rpm for 15 minutes to obtain a precursor solution; the mixed solution was prepared by mixing hydrofluoric acid and distilled water at a volume ratio of 1:25;

[0041] S2: Filter the precursor solution with filter paper, and let the filtrate stand at room temperature for 5 days;

[0042] S3: Collect the precipitated crystals, and rinse them with distilled water and ethanol three times respectively.

[0043] Experimental example

[0044] The performance of the birefringent crystals prepared in Examples 1 to 3 is similar, and the performance is described by taking the birefringent crystal in Example 1 as an example.

[0045] 1. Birefringent crystal SbTeO 3 Structural analysis of F

[0046] Birefringent Crystal SbTeO 3 The crystallographic data of F are shown in Table 1.

[0047] Table 1 Birefringent crystal SbTeO 3 Crystallographic data of F

[0048]

[0049] Note: a R 1 (F) = ∑||F o |-|F c || / ∑|F o |.wR 2 (F o 2 )=[∑w(F o 2 -F c 2 ) 2 / ∑w(F o 2 ) 2 ] 1 / 2

[0050] Compound SbTeO 3 F crystallizes in the orthorhombic system with a space group of P2 1 2 1 2 1 , the unit cell parameters are α=90°,β=90°,γ=90°,Z=4. Birefringent crystal SbTeO 3 The formation process of F Figure 1 As shown, it can be seen that in SbTeO 3 The F asymmetric unit contains an independent Sb atom, an independent Te atom, three independent O atoms, and an independent F atom; each Sb atom coordinates with three O atoms and one F atom to form a distorted [SbO 3 F] 4- Tetrahedral group ( Figure 1 a), where the Sb-O and Sb-F bond lengths range from 1.991(5) to 2.292(5) and 2.055(4), respectively; each Te atom coordinates with three O atoms to form a trigonal pyramidal [TeO 3 ] 3- Group ( Figure 1 a), whose bond length ranges from 1.886(5) to 1.913(5); [SbO 3 F] 4- Group and [TeO 3 ] 3- The groups are connected by shared O atoms to form a three-dimensional framework structure with alternating arrangements of 4-MRs and 8-MRs ( Figure 1 b).

[0051] 2. Birefringent crystal SbTeO 3 Characterization of F

[0052] (1) Birefringent crystal SbTeO 3 X-ray powder diffraction analysis of F

[0053] Figure 2 For birefringent crystal SbTeO 3 X-ray powder diffraction pattern of F; As can be seen from the figure, the XRD pattern of the experimental test is basically consistent with the XRD pattern of the single crystal fitting, indicating that SbTeO 3 Sample F is pure phase and can be tested in the next step. It also shows that the single crystal structure analysis is correct. 3 After the F sample was placed in air and water for 120 hours, the XRD test was performed again. It can be seen that the XRD spectrum has basically not changed, indicating that the compound SbTeO 3 F has good physical and chemical stability.

[0054] (2) Birefringent crystal SbTeO 3 Thermogravimetric analysis of F

[0055] Birefringent Crystal SbTeO 3 Thermogravimetric spectrum of F is shown in Figure 3 As shown in the figure, the birefringent crystal SbTeO 3 F can remain stable within 146℃ and begins to lose weight within the range of 146℃~800℃, with a total weight loss rate of 19.7%.

[0056] (3) Birefringent crystal SbTeO 3 Infrared spectrum analysis of F

[0057] Birefringent Crystal SbTeO 3 The infrared spectrum of F is as follows Figure 4 As shown in the figure, the birefringent crystal SbTeO 3 F has 4000~800cm -1 The wide window appears at 744cm -1 / 624cm -1 The peak at 509 cm is the asymmetric stretching vibration of Sb-O / F bond and Te-O bond. -1 The peaks at are the bending vibrations of the Sb-O / F bonds and the Te-O bonds.

[0058] (4) Birefringent crystal SbTeO 3 Analysis of UV-Vis diffuse reflectance spectrum of F

[0059] Birefringent Crystal SbTeO 3 The UV-visible diffuse reflectance of F is as follows Figure 5 As shown in the figure, SbTeO 3The experimental band gap of F is 4.08 eV, and the corresponding ultraviolet absorption cutoff edge is 303 nm. The results show that SbTeO 3 F is an ultraviolet optical material with application prospects.

[0060] (5) Birefringent crystal SbTeO 3 F birefringence test

[0061] Refractive crystal SbTeO measured with a ZEISS Axio A1 polarizing microscope at a wavelength of 546 nm 3 The birefringence of F is as follows: Figure 6 The test results show that the compound SbTeO 3 F exhibits a large birefringence of 0.298@546nm, indicating that SbTeO 3 F is an excellent birefringent material.

[0062] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A birefringent crystal, Features: The chemical formula of the birefringent crystal is SbTeO 3 F; the space group of the birefringent crystal is P2 1 2 1 2 1 ; The unit cell parameters are α=90°, β=90°, γ=90°, Z=4.

2. The method for preparing the birefringent crystal according to claim 1, It is characterized in that The following steps are involved: S1: mixing an antimony-containing compound and a tellurium-containing compound, dissolving the mixture in a mixed solution, and stirring at a stirring rate of 800 to 1200 rpm for 15 to 25 minutes to obtain a precursor solution; the mixed solution is obtained by mixing hydrofluoric acid and distilled water; S2: filtering the precursor solution, and allowing the obtained filtrate to stand at room temperature for 4 to 5 days; S3: Collect the precipitated crystals and wash them to obtain the product.

3. The preparation method according to claim 2, Features: The antimony-containing compound is SbF 3 , the tellurium-containing compound is TeO 2 .

4. The preparation method according to claim 3, Features: The SbF 3 and TeO 2 The molar ratio is 4:

1.

5. The preparation method according to claim 4, Features: The solid-liquid ratio of the mixture to the mixed solution is 1 g: 3-5 mL.

6. The preparation method according to claim 1 or 4, Features: The mixed solution is prepared by mixing hydrofluoric acid and distilled water in a volume ratio of 1:25 to 35.

7. The preparation method according to claim 6, Features: The mixed solution is prepared by mixing hydrofluoric acid and distilled water in a volume ratio of 1:

30.

8. The preparation method according to claim 2, Features: The stirring rate in S1 was 1000 rpm and the stirring time was 20 min.

9. The preparation method according to claim 2, Features: The cleaning method in S3 is to rinse with distilled water and ethanol 1 to 3 times respectively.

Citation Information

Patent Citations

  • Birefringent crystal and preparation method thereof

    CN114277444A

  • Tellurium molybdate birefringent crystal material and preparation and application thereof

    CN117448967A

  • Al2Te2MoO10 compound, Al2Te2MoO10 birefringent crystal, and preparation method and application of Al2Te2MoO10 birefringent crystal

    CN118374879A

Cited By

  • Tellurium-based optical crystal material with large birefringence as well as preparation method and application of tellurium-based optical crystal material

    CN119663451A