Method for preparing hydrophobic paper by utilizing eutectic solvent in combination with microwaves

By combining eutectic solvent with microwave heating pretreatment and hot pressing, cellulose paper with high mechanical strength, flexibility and hydrophobic properties is prepared, which solves the problems of complex and high cost of the existing superhydrophobic paper preparation process and realizes the Environmentally friendly and efficient hydrophobic paper production.

CN119061729AActive Publication Date: 2024-12-03QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411428414.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-03
Estimated Expiration
2044-10-14

AI Technical Summary

Technical Problem

The preparation process of existing superhydrophobic paper is complex, time-consuming and energy-consuming, and the resin needs to be modified and processed, and the synthesis process is relatively expensive, which loses the advantages of wood cell wall structure.

Method used

Basa wood was pretreated by eutectic solvent and microwave heating, and the fiber bonding strength was enhanced by TEMPO oxidation and AlCl3 cross-linking, and dense cellulose paper was prepared in combination with top-down hot pressing method, and the hydrophobic material HDTMS was coated by CVD method. Achieving hydrophobic paper preparation without polymer matrix.

Benefits of technology

It realizes the rapid, simple and efficient preparation of cellulose paper with high mechanical strength and flexibility and good hydrophobic properties, and the process is environmentally friendly and does not require the use of organic solvents, which reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061729A_ABST
    Figure CN119061729A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of new material development, in particular to a method for preparing hydrophobic paper by using a deep eutectic solvent in combination with microwaves. According to the method, balsa wood is used as a base material, microwave-assisted heating is adopted for pretreatment of a choline chloride-organic carboxylic acid eutectic solvent to quickly remove part of lignin in the wood, an obtained sample is subjected to hot-pressing treatment to prepare lignin-based paper, and finally hydrophobic hexadecyl trimethoxy silane molecules are coated through chemical vapor deposition to obtain the lignin-based paper. The hydrophobic paper with high mechanical strength, hydrophobicity and no polymer matrix is obtained. According to the prepared lignin-containing base hydrophobic paper, the tensile strength ranges from 11.3 Mpa to 25.4 Mpa, and the water contact angle ranges from 97.8 degrees to 101.6 degrees. The preparation method disclosed by the invention has the advantages of rapidness, feasibility, environment friendliness, low cost and the like. The prepared hydrophobic paper has wide application prospects in the fields of packaging, food, building materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new material development, and in particular to a method for preparing hydrophobic paper by utilizing a low eutectic solvent in combination with microwaves. Background Art

[0003] Super-hydrophobic paper refers to the hydrophobic paper whose contact angle formed when the paper surface contacts water is greater than 150° and whose rolling angle is less than 10°. The use of green and renewable hydrophobic paper as packaging material has broad development prospects; and super-hydrophobic paper has the properties of self-cleaning and anti-corrosion, and also has great application prospects in industrial production.

[0004] At present, super-hydrophobic paper is mainly prepared by coating, spraying or impregnating low surface energy materials with micro-nano structures. For example, the patent application number is 201210286775.0, which mentions the method for preparing a super-hydrophobic coating based on super-hydrophobic silica and resin. The resin is coated on a glass slide as a substrate, and the super-hydrophobic silica is adhered to the resin. After the resin is cured, the super-hydrophobic coating is obtained. However, the resin needs to be modified, the synthesis process is complicated, and the scope of application is narrow, and the comprehensive cost is relatively high; but the preparation process and procedure are relatively complicated, time-consuming and energy-consuming, and the structural advantages of the wood cell wall structure are lost during the pulping process. Summary of the invention

[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing hydrophobic paper using a low eutectic solvent combined with microwaves. The present invention uses environmentally friendly and renewable balsa wood as raw material, uses microwave-assisted heating of a low eutectic solvent to quickly remove part of the lignin in the wood, and the obtained sample is hot-pressed to prepare cellulose paper containing lignin in one step using a top-down method, which is simple, efficient, convenient and fast; finally, a hydrophobic material HDTMS is coated by a CVD method to obtain a cellulose paper-based material with high mechanical strength, good flexibility, hydrophobicity and no polymer matrix.

[0006] Application of the above hydrophobic paper.

[0007] To achieve the above object, the present invention adopts the following technical solutions: A method for preparing hydrophobic paper by using a deep eutectic solvent combined with microwaves, the method comprising the following steps: (1) mixing choline chloride and a hydrogen bond donor to obtain a DES solution; (2) adding balsa wood to the DES solution obtained in step (1), heating the solution for reaction, and using the treated balsa wood; (3) soaking the balsa wood obtained in step (2) in a sodium phosphate (PBS) solvent, adding TEMPO, sodium chlorite and sodium hypochlorite PBS solution, stirring, and reacting in a water bath to obtain oxidized balsa wood; (4) washing the oxidized balsa wood chips obtained in step (3), soaking them in an AlCl3 solution, and then hot pressing them to obtain a dense paper sample; (5) HDTMS (hexadecyltrimethoxysilane) is coated on the surface of the paper sample obtained in step (4) by chemical vapor deposition (CVD), and after drying, a hydrophobic paper sample is obtained.

[0008] Furthermore, in step (1), the hydrogen bond donor is at least one of oxalic acid, malonic acid, glutaric acid, lactic acid, malic acid and citric acid.

[0009] Furthermore, in step (1), the molar ratio of choline chloride to the hydrogen bond donor is 1:(1-3).

[0010] Furthermore, in step (1), the mixing is carried out at 60-120°C.

[0011] Furthermore, in step (2), the solid-liquid mass ratio of the balsa wood to the DES solution is 1:(20-40).

[0012] Furthermore, in step (2), the heating method is microwave heating.

[0013] Furthermore, the microwave heating has a power of 800-900 W and a heating time of 10-40 min.

[0014] Furthermore, in step (2), the heating reaction further requires washing the balsa wood with deionized water until the pH of the washed liquid is neutral, thereby obtaining treated balsa wood.

[0015] Furthermore, in step (3), the concentration of the sodium phosphate solvent is 0.5-2 M.

[0016] Furthermore, in step (3), the mass volume ratio of balsamic wood, sodium phosphate solvent, TEMPO, sodium chlorite and sodium hypochlorite PBS solution is (0.6-1.5) g: (100-300) mL: (0.02-0.04) g: (1.5-2.5) g: (10-20) mL.

[0017] Furthermore, the concentration of the sodium hypochlorite PBS solution is 0.05-0.2 M.

[0018] Furthermore, the temperature of the water bath reaction is 60-80°C and the time is 40-48 h.

[0019] Furthermore, in step (4), the cleaning reagent is deionized water.

[0020] Furthermore, in step (4), the mass fraction of the AlCl3 solution is 1-2 wt%.

[0021] Furthermore, in step (4), the soaking time is 20-30 h.

[0022] Furthermore, in step (4), the hot pressing pressure is 0.8-1.5 MPa, the time is 0.5-3 h, and the temperature is 90-100°C.

[0023] Furthermore, in step (5), the drying temperature is 150-165° C. and the drying time is 2-6 h.

[0024] The hydrophobic paper prepared by the above method.

[0025] The application of the hydrophobic paper is that the hydrophobic paper can be used in the fields of packaging, video, building materials, etc.

[0026] The present invention uses a low eutectic solvent of choline chloride and organic carboxylic acid to perform microwave-assisted heating pretreatment on balsa wood chips to remove part of the lignin, and then further enhances the bonding strength between the fibers through TEMPO oxidation and AlCl3 cross-linking, and then uses top-down hot pressing to prepare dense cellulose-based paper, in which neatly arranged cellulose fibers are retained, which helps to form a dense and neat structure, and the structure has higher mechanical strength and flexibility than wood with lignin removed.

[0027] Beneficial effects: The present invention uses a low eutectic solvent combined with microwaves to quickly remove lignin from plant fiber raw materials, and then uses a simple "top-down" hot pressing method to prepare dense cellulose paper with good mechanical properties; the obtained paper sample is coated with a hydrophobic HDTMS material using CVD, and the process does not require the use of organic solvents, which is green and environmentally friendly, and finally obtains a hydrophobic paper material with high mechanical strength, good hydrophobic properties, and no polymer matrix. The research and development of this new type of cellulose paper material has important environmental protection and application prospects, and plays an important role in improving the competitiveness of my country's core paper technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention, and the exemplary embodiments of the present invention and their description are used to explain the present invention, and do not constitute an improper limitation of the present invention.

[0029] Figure 1 The macroscopic morphology and flexibility display diagram of the hydrophobic paper prepared in Example 1 are shown in FIG. Figure 1 a is the macroscopic morphology, Figure 1 b is a diagram showing flexibility; Figure 2 The scanning electron microscope images of the hydrophobic paper prepared in Example 1 and Example 4 are shown in FIG. Figure 2 a is a scanning electron microscope image of the sample of Example 1, Figure 2 b is the scanning electron microscope image of the sample of Example 4; Figure 3 The infrared spectra of the hydrophobic paper prepared in Examples 1-4; Figure 4 The stress-strain curve diagram of the hydrophobic paper prepared in Examples 1-4; Figure 5 The water contact angle diagram of the hydrophobic paper prepared in Examples 1-4 is shown in FIG. Figure 5 a is the water contact angle diagram of the hydrophobic paper prepared in Example 1, Figure 5 b is the water contact angle diagram of the hydrophobic paper prepared in Example 2, Figure 5 c is the water contact angle diagram of the hydrophobic paper prepared in Example 3, Figure 5 d is the water contact angle diagram of the hydrophobic paper prepared in Example 4. Specific embodiments The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0031] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only. The present invention is further described according to the accompanying drawings and specific embodiments of the specification.

[0032] Example 1 (1) Choline chloride and oxalic acid were mixed in a molar ratio of 1:1, and stirred at 80° C. to form a transparent and stable solution, thereby preparing a DES solution; (2) adding balsa wood (5-10 mm in thickness) to the DES solution obtained in step (1) at a solid-liquid mass ratio of 1:30, and heating the mixture with microwave assistance for 10 min at a microwave power of 800 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (3) Soaking the balsa wood obtained in step (2) in a 0.1 M sodium phosphate (PBS) solvent (160 mL, pH 6.8), then adding 0.0256 g of TEMPO, 1.808 g of sodium chlorite and a 0.1 M sodium hypochlorite PBS solution (16 mL), stirring evenly, and reacting in a 60° C. water bath for 48 h to obtain oxidized balsa wood; (4) The oxidized balsa wood chips obtained in step (3) were washed with deionized water, and then immersed in a 1.5 wt% AlCl3 solution for 24 h, and then the immersed wood chip samples were hot pressed at a pressure of 1 MPa for 1 h at a temperature of 100 °C to obtain a dense paper sample; (5) HDTMS was coated on the surface of the paper sample obtained in step (4) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker and placed in an oven for drying at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0033] Example 2 (1) Choline chloride and oxalic acid were mixed in a molar ratio of 1:1, and stirred at 80° C. to form a transparent and stable solution, thereby preparing a DES solution; (2) adding balsa wood (thickness of 5-10 mm) to the DES solution obtained in step (1) at a solid-liquid ratio of 1:30, and heating with microwave assistance for 20 min at a microwave power of 800 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (3) Soak the balsa wood obtained in step (2) in 0.1 M sodium phosphate (PBS) solvent (160 mL, pH 6.8), then add 0.0256 g of TEMPO, 1.808 g of sodium chlorite and 0.1 M sodium hypochlorite PBS solution (16 mL), stir evenly, and place in a water bath at 60° C. for reaction for 48 h to obtain oxidized balsa wood chips; (4) The oxidized balsa wood chips obtained in step (3) were washed with deionized water and then immersed in a 1.5 wt % AlCl 3 solution for 24 h. The immersed wood chip samples were then hot pressed at a pressure of 1 MPa for 1 h at a temperature of 100 ° C to obtain a dense paper sample.

[0034] (5) HDTMS was coated on the surface of the dense paper sample obtained in step (4) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker, placed in an oven, and then dried at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0035] Example 3 (1) Choline chloride and oxalic acid were mixed in a molar ratio of 1:1, and stirred at 80° C. to form a transparent and stable solution, thereby preparing a DES solution; (2) adding balsa wood (5-10 mm in thickness) to the DES solution obtained in step (1) at a solid-liquid mass ratio of 1:30, and heating the mixture with microwave assistance for 30 min at a microwave power of 900 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (3) Soak the balsa wood obtained in step (2) in 0.1 M sodium phosphate (PBS) solvent (160 mL, pH 6.8), then add 0.0256 g of TEMPO, 1.808 g of sodium chlorite and 0.1 M sodium hypochlorite PBS solution (16 mL), stir evenly, place in a 60° C. water bath, and react for 48 h to obtain oxidized balsa wood; (4) The oxidized balsa wood chips obtained in step (3) were washed with deionized water, and then immersed in a 1.5 wt% AlCl3 solution for 24 h, and then the immersed wood chip samples were hot pressed at a pressure of 1 MPa for 1 h at a temperature of 100 °C to obtain a dense paper sample; (5) HDTMS was coated on the surface of the paper sample obtained in step (4) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker and placed in an oven for drying at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0036] Example 4 (1) preparing a DES solution by mixing choline chloride and oxalic acid in a molar ratio of 1:1, stirring at 80° C. to form a transparent and stable solution, thereby preparing a DES solution; (2) adding balsa wood (5-10 mm in thickness) to the DES solution obtained in step (1) at a solid-liquid mass ratio of 1:30, and heating the mixture with microwave assistance for 40 min at a microwave power of 900 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (3) Soaking the balsa wood obtained in step (2) in 0.1 M sodium phosphate (PBS) solvent (160 mL, pH 6.8), then adding 0.0256 g of TEMPO, 1.808 g of sodium chlorite and 0.1 M sodium hypochlorite PBS solution (16 mL), stirring evenly, and placing in a 60° C. water bath for reaction for 48 h to obtain oxidized balsa wood; (4) The oxidized balsa wood chips obtained in step (3) were washed with deionized water, and then immersed in a 1.5 wt% AlCl3 solution for 24 h, and then the immersed wood chip samples were hot pressed at a pressure of 1 MPa for 1 h at a temperature of 100 °C to obtain a dense paper sample; (5) HDTMS was coated on the surface of the paper sample obtained in step (4) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker and placed in an oven for drying at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0037] Comparative Example 1 (1) preparing a DES solution by mixing choline chloride and oxalic acid in a molar ratio of 1:1, stirring at 80° C. to form a transparent and stable solution, thereby preparing a DES solution; (2) adding balsa wood (5-10 mm in thickness) to the DES solution obtained in step (1) at a solid-liquid mass ratio of 1:30, and heating the mixture with microwave assistance for 30 min at a microwave power of 900 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (3) Soak the balsa wood obtained in step (2) in 0.1 M sodium phosphate solvent (160 mL, pH 6.8), then add 0.0256 g of TEMPO, 1.808 g of sodium chlorite and 16 mL of 0.1 M sodium hypochlorite PBS solution, stir evenly, and place in a 60° C. water bath for reaction for 48 h to obtain oxidized balsa wood; (4) washing the oxidized balsa wood chips obtained in step (3) with deionized water, and then hot pressing the washed wood chip samples at a pressure of 1 MPa for 1 h at a temperature of 100° C. to obtain a dense paper sample; (5) HDTMS was coated on the surface of the paper sample obtained in step (4) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker and placed in an oven for drying at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0038] The tensile strength of the hydrophobic paper obtained in Comparative Example 1 is 16.1 MPa, and the elongation at break is 2.48%.

[0039] Comparative Example 2 (1) adding balsa wood (5-10 mm thick) into deionized water at a solid-liquid mass ratio of 1:30, and heating with microwave assistance for 30 min at a microwave power of 900 W. After the reaction is completed, rinsing the balsa wood with deionized water until the pH of the rinsed liquid is neutral, thereby obtaining treated balsa wood; (2) Soaking the balsa wood obtained in step (1) in 0.1 M sodium phosphate (PBS) solvent (160 mL, pH 6.8), then adding 0.0256 g of TEMPO, 1.808 g of sodium chlorite and 0.1 M sodium hypochlorite PBS solution (16 mL), stirring evenly, and reacting in a 60° C. water bath for 48 h to obtain oxidized balsa wood; (3) The oxidized balsa wood chips obtained in step (2) were washed with deionized water, and then immersed in a 1.5 wt% AlCl3 solution for 24 h, and then the immersed wood chip samples were hot pressed at a pressure of 1 MPa for 1 h at a temperature of 100°C to obtain a dense paper sample; (4) HDTMS was coated on the surface of the paper sample obtained in step (3) by a CVD method. The paper sample coated with HDTMS was stored in a glass beaker, placed in an oven, and dried at 155° C. for 3 h to obtain a hydrophobic paper sample.

[0040] The tensile strength of the hydrophobic paper obtained in Comparative Example 2 is 18.6 MPa, and the elongation at break is 1.94%.

[0041] It can be clearly found from Comparative Examples 1 and 2 that microwave-assisted heating of low eutectic solvent pretreatment and AlCl3 crosslinking can further improve the mechanical strength and flexibility of the hydrophobic paper.

[0042] Performance Testing Figure 1 The macroscopic morphology and flexibility of the hydrophobic paper prepared in Example 1 are shown in FIG. Figure 1 a is the macroscopic morphology, Figure 1 b is a diagram showing flexibility. The results show that the macroscopic morphology of the hydrophobic paper obtained in Example 1 is dark yellow in color and can be wrapped around a pen without breaking, indicating that the cellulose paper has good flexibility.

[0043] Figure 2 The scanning electron microscope images of the hydrophobic paper prepared in Example 1 and Example 4 are shown in FIG. Figure 2 a is a scanning electron microscope image of the sample of Example 1, Figure 2 b is the scanning electron microscope image of the sample in Example 4. Detection method: The sample was placed on a sample stand with a conductive double-sided tape, and after gold was sprayed using an Oxford Quorum SC7620 sputtering coater, the surface morphology of the sample was photographed using a TESCAN MIRA LMS scanning electron microscope. The results showed that as the DES treatment time of the sample increased, the surface morphology roughness of the prepared cellulose paper gradually increased, indicating that DES treatment can remove components such as lignin in the cell wall of balsa wood, resulting in a rough and uneven surface morphology in the image.

[0044] Figure 3The infrared spectrum of the hydrophobic paper prepared in Example 1-4. Detection method: ALPHA infrared tester was used to detect in ATR mode. -1 The absorption peak at 1507cm is the stretching vibration peak of C=O in lignin. -1 The absorption peak at is the stretching vibration peak of the lignin benzene ring skeleton. It can be seen from the figure that the sample after DES treatment still contains a certain amount of lignin, and with the increase of microwave heating time, its peak intensity gradually weakens, indicating that with the increase of treatment time, the content of lignin gradually decreases.

[0045] Figure 4 The stress-strain curve of the hydrophobic paper prepared in Example 1-4. Detection method: Use a texture analyzer to measure the physical strength properties of paper, set the test speed to 19.8 mm / min, and record the stress-strain curve. The tensile strength of the hydrophobic paper of Example 1-4 is 25.4 MPa, 20.1 MPa, 17.2 MPa and 11.3 MPa, respectively, and the elongation at break is 1.86%, 2.25%, 2.78%, and 1.38%, respectively. The results show that with the increase of the treatment time of the low eutectic solvent, the tensile strength gradually decreases; the elongation at break first increases and then decreases. After 30 min microwave reaction, its elongation at break is the highest, indicating that the hydrophobic paper is easier to bend and has better flexibility. This is because the longer the DES treatment time, the more lignin is removed; and lignin has a certain rigidity and adhesiveness. The presence of an appropriate amount of lignin can play a reinforcing role in cellulose paper, but too much lignin will affect the flexibility of the hydrophobic paper.

[0046] Figure 5 The water contact angle diagram of the hydrophobic paper prepared in Examples 1-4 is shown in FIG. Figure 5 a is the water contact angle diagram of the hydrophobic paper prepared in Example 1, Figure 5 b is the water contact angle diagram of the hydrophobic paper prepared in Example 2, Figure 5 c is the water contact angle diagram of the hydrophobic paper prepared in Example 3, Figure 5 d is the water contact angle diagram of the hydrophobic paper prepared in Example 4. Detection method: The water contact angle of the sample was measured using a fully automatic video optical contact angle meter (OCA50). The cellulose paper samples that were treated with DES microwave heating for 10 min, 20 min, 30 min, and 40 min and then hydrophobically modified were tested for contact angle. The results showed that the contact angles of the hydrophobic papers prepared in Examples 1-4 were 101.6°, 101.1°, 99.3°, and 97.8°, respectively, indicating that with the increase of DES pretreatment time, the contact angle of the HDTMS-modified hydrophobic paper gradually decreased. The possible reason is that with the increase of microwave heating pretreatment time, the hydrophobic lignin content in the cellulose paper gradually decreased, resulting in a gradual decrease in the hydrophobic angle.

[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing hydrophobic paper using a deep eutectic solvent combined with microwaves, characterized in that: The method comprises the following steps: (1) mixing choline chloride and a hydrogen bond donor organic carboxylic acid to obtain a DES solution; (2) adding balsa wood to the DES solution obtained in step (1), heating the solution for reaction, and using the treated balsa wood; (3) soaking the balsa wood obtained in step (2) in a sodium phosphate solvent, adding TEMPO, sodium chlorite and sodium hypochlorite PBS solution, stirring, and reacting in a water bath to obtain oxidized balsa wood; (4) washing the oxidized balsa wood chips obtained in step (3), soaking them in an AlCl3 solution, and then hot pressing them to obtain a dense paper sample; (5) HDTMS is coated on the surface of the paper sample obtained in step (4) by a CVD method, and after drying, a hydrophobic paper sample is obtained.

2. The method according to claim 1, characterized in that In step (1), the hydrogen bond donor is at least one of oxalic acid, malonic acid, glutaric acid, lactic acid, malic acid and citric acid; The molar ratio of the choline chloride to the hydrogen bond donor is 1:(1-3).

3. The method according to claim 1, characterized in that In step (2), the solid-liquid mass ratio of the balsa wood to the DES solution is 1:(20-40); The heating method is microwave heating.

4. The method according to claim 3, characterized in that The microwave heating has a power of 700-1000 W and a heating time of 5-60 min.

5. The method according to claim 1, characterized in that In step (2), the heating reaction further requires washing the balsa wood with deionized water until the pH of the washed liquid is neutral, thereby obtaining the treated balsa wood.

6. The method according to claim 1, characterized in that In step (3), the concentration of the sodium phosphate solvent is 0.5-2 M; The concentration of the sodium hypochlorite PBS solution is 0.05-0.2 M; The mass volume ratio of the balsamic wood, sodium phosphate solvent, TEMPO, sodium chlorite and sodium hypochlorite PBS solution is (0.6-1.5) g: (100-300) mL: (0.02-0.04) g: (1.5-2.5) g: (10-20) mL; The temperature of the water bath reaction is 60-80° C. and the reaction time is 40-48 h.

7. The method according to claim 1, characterized in that In step (4), the cleaning reagent is deionized water; The mass fraction of the AlCl3 solution is 1-2 wt%; The soaking time is 20-30 h; The hot pressing pressure is 0.8-1.5 MPa, the time is 0.5-3 h, and the temperature is 90-100°C.

8. The method according to claim 1, characterized in that In step (5), the drying temperature is 150-165° C. and the drying time is 2-6 h.

9. The hydrophobic paper prepared by the method described in any one of claims 1 to 8.

10. Use of the hydrophobic paper prepared by the method according to any one of claims 1 to 8 and / or the hydrophobic paper according to claim 9, characterized in that: The hydrophobic paper is used in the fields of packaging, food and building materials.

Citation Information

Patent Citations

  • Preparation method of elastic wood, prepared elastic wood and application of elastic wood

    CN110978180A

  • Preparation method of ultrathin wood vibrating diaphragm

    CN113547598A

  • Technology for making compound ceramic-wood material and its product

    CN1263810A

  • Delignification of materials in deep eutectic solvents

    US20240328084A1

  • Method for the chemically assisted mechanical pulping of wood chips or wood shavings

    WO2022170373A1