Method for improving mechanical stress side effect caused by volume expansion of silicon-based anode

By using porous graphite @silicon-carbon nanotubes as anode material in lithium-ion batteries, the mechanical stress problem caused by volume expansion of silicon-based anode is solved, the cycle stability and specific capacity of the battery are improved, and more efficient charge transmission is achieved and conductivity.

CN119069685APending Publication Date: 2024-12-03JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411285126.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The side effects of mechanical stress caused by volume expansion in silicon-based anodes in lithium-ion batteries lead to unstable electrode structure and attenuation of performance, and the high surface energy of nano-silicon particles leads to an increase in aggregation and transmission resistance, affecting battery performance.

Method used

Porous graphite @ silicon-carbon nanotubes are used as the anode active material, and prepared by spray drying and firing processes. The porous carbon structure is used to limit the movement and aggregation of nanosilicon particles, providing buffer space and conductive channels, improving the stability and conductivity of the electrode sex.

Benefits of technology

It effectively alleviates the damage to the electrode structure by volume expansion, improves the cycle stability and specific capacity of the battery, reduces the side effects caused by mechanical stress, and improves the charge transfer efficiency and material circulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of anode materials, in particular to a method for improving mechanical stress side effects caused by volume expansion of a silicon-based anode. The method is realized by preparing a porous graphite and silicon-carbon nanotube as an anode active material. According to the invention, graphite and nano silicon particles are used as main electroactive components of an anode, and then the graphite, the nano silicon particles, citric acid and asphalt are fired and pyrolyzed to prepare the porous graphite at silicon-carbon nanotube. The porous graphite at silicon-carbon nanotube can be used as a silicon-based anode to improve volume expansion in charge and discharge processes, so that side effects caused by mechanical stress are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anode materials, and in particular to a method for improving the side effects of mechanical stress caused by volume expansion of a silicon-based anode. Background Art

[0002] In recent years, lithium-ion batteries have become increasingly important due to their large-scale application in electrochemical energy storage and power batteries for electric vehicles (EVs) and hybrid electric vehicles (HEVs). Carbon and graphite are the most commonly used negative electrode materials for commercial lithium-ion batteries due to their low price, high conductivity and good stability. However, the theoretical capacity of graphite is relatively low, only 372 mAh g -1 , which greatly limits its further application in high-power systems such as electric vehicles and hybrid vehicles. Therefore, new anode materials with high capacity and long life have received extensive attention and research around the world.

[0003] The theoretical specific capacity of silicon-based anode materials is as high as 4200 mAh g -1 , and pure silicon is stable and has a low original potential (~0.4V), so it is considered to be an ideal substitute for carbon and graphite. However, the volume change of silicon-based anodes during the lithium insertion and extraction process is greater than 300%. Excessive volume change will cause high mechanical stress, which will cause the active particles to pulverize, thereby destroying the integrity of the electrode structure; at the same time, it will also destroy the SEI film on the silicon surface, causing the exposed silicon surface to directly contact the electrolyte, and then the repeated growth of the SEI film, resulting in the insulation of the pulverized silicon particles, and the loss of electrical contact with the current collector, which ultimately causes the performance of silicon-based lithium-ion batteries to continue to decay. Therefore, people have been working hard to improve the electrochemical performance of silicon-based anodes. Using silicon nanocrystals as silicon-based anode materials is considered to be an effective method. However, the surface energy of nano-silicon particles is very high, making them easy to aggregate together, which will increase the internal transmission resistance of the electrode and affect the battery performance. Therefore, how to improve the dispersibility of nano-silicon particles has become a key challenge for the actual use of silicon-based anodes in lithium-ion batteries.

[0004] In summary, the present invention provides a method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes, which is of great significance. Summary of the invention

[0005] The object of the present invention is to provide a method for improving the side effects of mechanical stress caused by volume expansion of a silicon-based anode, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes is achieved by using porous graphite@silicon-carbon nanotubes as anode active materials.

[0007] Furthermore, the method for preparing the porous graphite@silicon-carbon nanotubes comprises the following steps: S1: Weigh graphite, nano-silicon particles and carbon source according to the designed mass ratio; S2: Weigh nano-silicon particles and polyvinyl pyrrolidone, add them to the ethanol solution, and ultrasonically vibrate for 30-90 minutes to obtain a uniform suspension; S3: adding the suspension obtained in S2 and graphite to a citric acid-ethanol solution, stirring magnetically for 30 to 90 minutes, and then spray drying to obtain a graphite / silicon / carbon organic precursor I; S4: placing the graphite / silicon / carbon organic precursor I obtained in S3 in a quartz tube furnace, heating it to 370-390°C under nitrogen protection, firing it for 3-6 hours, stopping the firing, and cooling it naturally to room temperature to obtain a graphite / silicon / carbon composite material I; S5: adding the graphite / silicon / carbon composite material I obtained in S4 to the asphalt-tetrahydrofuran solution, stirring magnetically for 30 to 90 minutes, and then spray drying to obtain a graphite / silicon / carbon organic precursor II; S6: placing the graphite / silicon / carbon organic precursor II obtained in S5 in a quartz tube furnace, heating it to 490-510°C under nitrogen protection, firing it for 3-6 hours, then heating it to 890-910°C, firing it for 3-6 hours, stopping firing, and cooling it naturally to room temperature, then grinding and sieving it to obtain a graphite / silicon / carbon composite material II; S7: Weigh ferric nitrate, aluminum nitrate and citric acid according to the designed molar ratio, add them into deionized water, stir and dissolve, heat to 100°C in a water bath, keep warm for 3-6 hours, stop heating, and finally allow to cool naturally to room temperature to obtain a Fe2O3-Al2O3 gel catalyst; S8: adding the graphite / silicon / carbon composite material II obtained in S6 to the ethanol solution, magnetically stirring for 30 to 90 minutes to make it evenly dispersed, then adding the Fe2O3-Al2O3 gel catalyst obtained in S7, continuing to stir for 10 to 20 minutes, and finally filtering and drying to obtain a graphite / silicon / carbon / catalyst composite material; S9: Place the graphite / silicon / carbon / catalyst composite material obtained in S8 in a quartz tube furnace, and under the protection of argon, heat it to 660-690°C, then introduce C2H2 into the quartz tube furnace, keep it warm for 15-45 minutes, stop firing, and finally allow it to cool naturally to room temperature to obtain porous graphite@silicon-carbon nanotubes.

[0008] Furthermore, the mass ratio of the graphite, nano-silicon particles and carbon source is 36:5:9.

[0009] Furthermore, the carbon source includes but is not limited to a combination of one or more of citric acid and asphalt.

[0010] Furthermore, the carbon source is a combination of citric acid and asphalt, and the mass ratio of the two is 10:3.

[0011] Furthermore, the mass ratio of the nano-silicon particles to polyvinyl pyrrole is 7:3.

[0012] Furthermore, the spray drying is carried out using a centrifugal atomizer; wherein the setting parameters of the centrifugal atomizer are: a rotation speed of 30,000-40,000 rpm, a delivery rate of 12-18 mL / min, an inlet temperature of 115-125° C., and an outlet temperature of 75-85° C.

[0013] Furthermore, the molar ratio of the ferric nitrate, aluminum nitrate and citric acid is 4:1:5.

[0014] Furthermore, the mass ratio of the graphite / silicon / carbon composite material II and the Fe2O3-Al2O3 gel catalyst is 5:1.

[0015] Since nano-silicon particles will move and aggregate violently during the volume change process, resulting in instability of the electrode structure and rapid degradation of performance, porous graphite@silicon-carbon nanotubes were prepared as anode active materials in the scheme. Porous graphite@silicon-carbon nanotubes have porous carbon with rich pore structures. These pore structures can, on the one hand, limit the excessive movement and agglomeration of nano-silicon particles to a certain extent, "fix" the nano-silicon particles, make them move within a certain range, and maintain the relative stability of the electrode structure; on the other hand, they can provide space for the volume expansion of nano-silicon particles, thereby effectively avoiding huge squeezing and damage to the electrode structure, and alleviating the overall volume change of the anode.

[0016] In addition, the good conductivity of porous carbon itself also helps to improve the performance of the silicon negative electrode, improve the electronic conductivity of the electrode, and make the charge transfer faster and more efficient. This also helps to alleviate the problems such as increased resistance due to volume expansion to a certain extent, and indirectly helps to suppress the negative impact of volume expansion on battery performance.

[0017] Compared with the prior art, the beneficial effects achieved by the present invention are: (1) The spray drying method is used repeatedly in the scheme, which is environmentally friendly, economical and has relatively high yield, and can achieve mass production; (2) Graphite and nano-silicon particles are the main electroactive components of the anode, while the porous carbon produced by pyrolysis of citric acid and asphalt has multiple functions, including serving as a matrix to accommodate silicon, providing a buffer space for silicon, serving as a barrier to inhibit the aggregation of nano-scale silicon, and providing a free channel for the penetration of liquid electrolyte, thereby maximizing the electroactive area of ​​graphite and silicon; (3) Graphite can also provide sufficient electrical conductivity and mechanical strength. Therefore, the porous graphite@silicon-carbon nanotubes prepared by the present invention have the characteristics of high electrical conductivity, high stability during the formation of the solid-electrolyte interface and good structural integrity. (4) The introduction of highly conductive carbon materials, porous carbon, can solve the problem of insufficient conductivity between particles, thereby improving the material's cycle stability and rate performance; (5) The porous graphite@silicon-carbon nanotubes prepared in the present invention can be used as a silicon-based anode to improve the volume expansion during the charge and discharge process, better play the advantages of high specific capacity materials such as silicon negative electrode, and improve the overall specific capacity of the battery, thereby reducing the side effects caused by mechanical stress. DETAILED DESCRIPTION

[0018] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.

[0019] Pre-preparation: 1. Prepare citric acid-ethanol solution: Mix 70 g / L citric acid solution and 95 wt % ethanol in a volume ratio of 10:1 to prepare a citric acid-ethanol solution.

[0020] 2. Preparation of asphalt-tetrahydrofuran solution: (1) Weigh coal tar pitch and tetrahydrofuran in a mass ratio of 1:10 and prepare them; (2) Place the coal tar pitch in a ground-mouth conical flask, slowly add tetrahydrofuran, and gently shake the conical flask to avoid splashing; (3) Place the ground-mouth conical flask on a magnetic stirrer, turn on the stirrer, and stir the mixture at a speed of 2000 r / min at room temperature for 5 hours to ensure that the coal tar pitch is fully dissolved in tetrahydrofuran; (4) Finally, remove the insoluble matter by filtration, collect the clear filtrate, and obtain the asphalt-tetrahydrofuran solution.

[0021] Example 1: A method for improving the mechanical stress side effects caused by the volume expansion of silicon-based anodes: S1: Weigh graphite, nano-silicon particles and carbon source in a mass ratio of 36:5:9; the carbon source is citric acid and asphalt in a mass ratio of 10:3; S2: Nano-silicon particles and polyvinyl pyrrolidone weighed in a mass ratio of 7:3 are added to a 95wt% ethanol solution and ultrasonically vibrated for 60 minutes to obtain a uniform suspension; S3: The suspension obtained in S2 and the weighed graphite were added to the citric acid-ethanol solution, and after magnetic stirring for 60 minutes, a centrifugal-atomizer was used for spray drying, and the parameters were set as follows: the rotation speed was 35000 rpm, the delivery rate was 15 mL / min, the inlet temperature was 120°C, and the outlet temperature was 80°C, to obtain a graphite / silicon / carbon organic precursor I; S4: placing the graphite / silicon / carbon organic precursor I obtained in S3 in a quartz tube furnace, heating it to 380° C. under nitrogen protection, firing it for 4 h, stopping the firing, and allowing it to cool naturally to room temperature to obtain a graphite / silicon / carbon composite material I; S5: adding the graphite / silicon / carbon composite material I obtained in S4 to the asphalt-tetrahydrofuran solution, stirring magnetically for 60 minutes, and then spray drying using a centrifugal-atomizer, with the following parameters set: rotation speed of 35000 rpm, delivery rate of 15 mL / min, inlet temperature of 120°C, outlet temperature of 80°C, to obtain a graphite / silicon / carbon organic precursor II; S6: placing the graphite / silicon / carbon organic precursor II obtained in S5 in a quartz tube furnace, heating it to 500°C under nitrogen protection, firing it for 4 hours, then heating it to 900°C and firing it for 4 hours, stopping firing, and cooling it naturally to room temperature, grinding and sieving it to obtain a graphite / silicon / carbon composite material II; S7: Weigh ferric nitrate, aluminum nitrate and citric acid in a molar ratio of 4:1:5, add the three into deionized water, stir and dissolve, heat in a water bath to 100°C, keep warm for 4 hours, stop heating, and finally cool naturally to room temperature to obtain a Fe2O3-Al2O3 gel catalyst; S8: adding the graphite / silicon / carbon composite material II obtained in S6 to the ethanol solution, magnetically stirring for 60 minutes to make it evenly dispersed, and then adding the Fe2O3-Al2O3 gel catalyst obtained in S7, wherein the mass ratio of the graphite / silicon / carbon composite material II to the Fe2O3-Al2O3 gel catalyst is 5:1, continuing to stir for 10 minutes, and finally filtering and drying to obtain a graphite / silicon / carbon / catalyst composite material; S9: The graphite / silicon / carbon / catalyst composite material obtained in S8 is placed in a quartz tube furnace. Under the protection of argon, the temperature is raised to 680°C, and then C2H2 is introduced into the quartz tube furnace at a rate of 20 mL / min. The temperature is kept for 30 minutes, and the firing is stopped. Finally, it is allowed to cool naturally to room temperature to obtain porous graphite@silicon-carbon nanotubes.

[0022] Based on Example 1, a control experiment was carried out, specifically Comparative Examples 1 to 3, as described below: Comparative Example 1: Comparative Example 1 is based on Example 1, with the following adjustments: the operations of S7 to S9 are not performed, and other processes remain unchanged, that is, graphite / silicon / carbon composite material II is used as the anode active material.

[0023] Comparative Example 2: Graphite is directly used as the anode active material; Comparative Example 3: Nano-silicon particles are directly used as the anode active material.

[0024] In the above examples, all raw materials come from the following sources: Graphite: Shanghai Aladdin Biochemical Technology Co., Ltd., purity: 99.95%; Nano silicon particles: Shanghai Aladdin Biochemical Technology Co., Ltd., purity: 99.99%; Citric acid: Suzhou Mingzhen Chemical Technology Co., Ltd.; Asphalt: Zhejiang Tuyue New Material Technology Co., Ltd.; Polyvinylpyrrolidone: Hubei Xinghengye Technology Co., Ltd.; Ferric nitrate: Guangdong Xinmo Chemical Co., Ltd.; Aluminum nitrate: Shanghai MacLean Biochemical Technology Co., Ltd.

[0025] Performance test: The anode active materials corresponding to Example 1 and Comparative Examples 1 to 3 were prepared into batteries, and then the charge and discharge performance tests were performed. The specific test method was as follows: (1) mixing an anode active material, acetylene black and polyvinyl difluoride in N-methylpyrrolidone at a mass ratio of 8:1:1, and mixing them evenly to obtain a slurry; (2) coating the slurry onto copper foil, placing it at 120°C and vacuum drying it for 12 hours to obtain an electrode sheet; (3) Cut the electrode sheet into 1.54cm 2 (1.4 cm in diameter) discs were compacted with a force of 400 N / cm to obtain electrode discs; the loading amount of the anode active material on the electrode discs was ensured to be 0.5 mg / cm 2 ; (4) In a glove box filled with high-purity argon (more than 99.5%), the electrode discs were assembled into CR2016 button cells, with lithium sheets as counter electrodes, polypropylene films as separators, and LiPF6 solution as electrolyte (the LiPF6 solution was obtained by mixing ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate in a volume ratio of 1:1:1, and adding 2 wt% of vinylene carbonate as an additive); (5) The battery charge and discharge performance was tested using a LANDCT2001A battery tester. Specifically, the battery specific capacity was tested after 100 cycles of charge and discharge at a current density of 0.5 A / g.

[0026] The specific test results are shown in Table 1 below: Table 1

[0027] Result analysis: According to the data in Table 1 above, it can be seen that the electrode cycle performance of the porous graphite@silicon-carbon nanotube (Example 1) prepared by the present invention as an anode active material is significantly improved compared with graphite (Comparative Example 2), nano silicon particles (Comparative Example 3) and graphite / silicon / carbon composite material II (Comparative Example 1); it shows that the anode active material prepared in Example 1 has a stable anode structure during the charge and discharge process, can effectively reduce the anode volume expansion, greatly reduce the loss of anode active materials caused by structural damage and the increase in electrode internal resistance, can better play the advantages of silicon negative electrode high specific capacity materials, and has a significant positive gain for the overall specific capacity of the battery. The improvement of the battery specific capacity in Example 1 can fully confirm that the anode volume expansion is reduced during the charge and discharge process.

[0028] In summary, when the volume expansion is reduced, the electrode structure can remain relatively stable during the charge and discharge process, and the loss of active materials in the electrode and the increase in internal resistance of the electrode are suppressed, so that the battery can perform charge and discharge reactions more effectively and give full play to the electrochemical properties of the active materials. For this reason, the battery's discharge specific capacity does not decay rapidly. For silicon negative electrodes, the volume expansion is extremely serious during the charge and discharge process; therefore, if the volume expansion can be reduced, the advantages of high specific capacity materials such as silicon negative electrodes can be better utilized to improve the overall specific capacity of the battery.

[0029] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.

Claims

1. A method for improving the mechanical stress side effects caused by the volume expansion of silicon-based anodes, characterized in that: This is achieved by using porous graphite@silicon-carbon nanotubes as the anode active material.

2. The method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes according to claim 1, characterized in that: The method for preparing the porous graphite@silicon-carbon nanotubes comprises the following steps: S1: weigh graphite, nano-silicon particles, and carbon source; S2: Add nano-silicon particles and polyvinyl pyrrolidone to the ethanol solution and ultrasonically vibrate for 30-90 minutes to obtain a uniform suspension; S3: adding the suspension obtained in S2 and graphite to a citric acid-ethanol solution, stirring magnetically for 30 to 90 minutes, and then spray drying to obtain a graphite / silicon / carbon organic precursor I; S4: placing the graphite / silicon / carbon organic precursor I obtained in S3 in a quartz tube furnace, heating it to 370-390°C under nitrogen protection, firing it for 3-6 hours, stopping the firing, and cooling it naturally to room temperature to obtain a graphite / silicon / carbon composite material I; S5: adding the graphite / silicon / carbon composite material I obtained in S4 to the asphalt-tetrahydrofuran solution, stirring magnetically for 30 to 90 minutes, and then spray drying to obtain a graphite / silicon / carbon organic precursor II; S6: placing the graphite / silicon / carbon organic precursor II obtained in S5 in a quartz tube furnace, heating it to 490-510°C under nitrogen protection, firing it for 3-6 hours, then heating it to 890-910°C, firing it for 3-6 hours, stopping firing, and cooling it naturally to room temperature, then grinding and sieving it to obtain a graphite / silicon / carbon composite material II; S7: Weigh ferric nitrate, aluminum nitrate and citric acid, add them to deionized water, stir and dissolve, heat to 100°C in a water bath, keep warm for 3-6 hours, stop heating, and finally allow to cool naturally to room temperature to obtain a Fe2O3-Al2O3 gel catalyst; S8: adding the graphite / silicon / carbon composite material II obtained in S6 to the ethanol solution, magnetically stirring for 30 to 90 minutes to make it evenly dispersed, then adding the Fe2O3-Al2O3 gel catalyst obtained in S7, continuing to stir for 10 to 20 minutes, and finally filtering and drying to obtain a graphite / silicon / carbon / catalyst composite material; S9: Place the graphite / silicon / carbon / catalyst composite material obtained in S8 in a quartz tube furnace, and under the protection of argon, heat it to 660-690°C, then introduce C2H2 into the quartz tube furnace, keep it warm for 15-45 minutes, stop firing, and finally allow it to cool naturally to room temperature to obtain porous graphite@silicon-carbon nanotubes.

3. The method for improving the mechanical stress side effect caused by the volume expansion of silicon-based anode according to claim 2, characterized in that: In S1, the mass ratio of the graphite, nano-silicon particles and carbon source is 36:5:9; wherein the carbon source includes a combination of one or more of citric acid and asphalt.

4. The method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes according to claim 3, characterized in that: The carbon source is a combination of citric acid and asphalt, and the mass ratio of the two is 10:

3.

5. The method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes according to claim 2, characterized in that: In S2, the mass ratio of the nano-silicon particles to polyvinyl pyrrolidone is 7:

3.

6. The method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes according to claim 2, characterized in that: In S3 and S5, the spray drying is carried out by a centrifugal atomizer; wherein the setting parameters of the centrifugal atomizer are: a rotation speed of 30,000-40,000 rpm, a delivery rate of 12-18 mL / min, an inlet temperature of 115-125° C., and an outlet temperature of 75-85° C.

7. The method for improving the side effects of mechanical stress caused by volume expansion of silicon-based anodes according to claim 2, characterized in that: In S7, the molar ratio of the ferric nitrate, aluminum nitrate and citric acid is 4:1:

5.