Polyvinyl alcohol-based composite material as well as preparation method and application thereof

By femtosecond laser treatment of titanium alloy matrix and combining with a polyvinyl alcohol-based polymer gel coating with a specific structure, the problem of insufficient bonding strength of the implant surface modification coating is solved, and long-lasting antibacterial and bone growth promotion effect is achieved. Suitable for orthopedic implants.

CN119074995AActive Publication Date: 2024-12-06HEBEI UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411232241.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The binding strength of existing implant surface modification coatings is insufficient, resulting in the inability to maintain biological functions for a long time, making it difficult to prevent implant-related infections and promote tissue repair.

Method used

Titanium alloy matrix treated with femtosecond laser, combined with a polyvinyl alcohol-based polymer gel coating with a specific structure, enhances antibacterial and osteogenic properties through the coordination and slow release of Cu2+, and uses trippyridine and catheterol Groups improve material stability and biocompatibility.

Benefits of technology

It significantly enhances the binding strength of the gel coating and the matrix, achieves a long-lasting antibacterial effect and promotes the bone growth environment, improves the biocompatibility and antibacterial properties of the material, and is suitable for orthopedic implants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119074995A_ABST
    Figure CN119074995A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyvinyl alcohol materials, and particularly discloses a polyvinyl alcohol-based composite material as well as a preparation method and application thereof. The titanium alloy matrix is subjected to surface treatment through a femtosecond laser technology, so that a unique micro-nano multilevel structure is generated on the surface of the titanium alloy, the bonding strength of gel and the titanium alloy matrix is enhanced, and a proper amount of copper ions are introduced into the polyvinyl alcohol-based polymer with a specific structure, so that the bonding strength of the gel and the titanium alloy matrix is improved. According to the present invention, with the introduction of the proper amount of Cu < 2 + >, the biocompatibility and the antibacterial property of the material can be improved, and the cytotoxic reaction and the protein adsorption induced by the high-concentration metal ions can be avoided so as to achieve the purposes of stable and lasting antibacterial property and bone cell directional differentiation promotion. The polyvinyl alcohol-based composite material is expected to bring a more reliable and lasting treatment effect to the fields of bone disease treatment and implant repair clinically, and has a wide application prospect in the field of bone repair implant materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyvinyl alcohol materials, and in particular to a polyvinyl alcohol-based composite material and a preparation method and application thereof. Background Art

[0002] In recent years, with the gradual increase in the use of implants, the risk of implant-related infection has become increasingly prominent. Implants are very likely to cause bacterially infected bone defects and chronic osteomyelitis. The occurrence of osteomyelitis is often accompanied by bacterial infection and the formation of biofilms, which leads to the interruption of the periosteum and intraosseous arterial system, and then causes bone necrosis. At present, the gold standard for the treatment of osteomyelitis is local antibiotic delivery combined with systemic antibiotic treatment, but the formation of biofilms limits the effectiveness of antibiotics, therefore, it is very easy to cause disease recurrence and difficult to treat. Therefore, prevention has become a key strategy in clinical practice.

[0003] At present, although pure titanium and its alloy materials widely used in clinical practice have good chemical stability, mechanical strength, corrosion resistance and biocompatibility, they lack antibacterial properties and are prone to bacterial infection, leading to secondary surgery and consuming a lot of resources. Staphylococcus aureus is the main pathogen of orthopedic implant infection. Although antibiotics have been widely studied, they are prone to drug resistance, especially multidrug resistance. In addition, researchers are committed to constructing coatings with immune-osteogenic regulatory functions on the surface of implants in order to achieve the dual effects of antibacterial and osteogenesis. Although research on the surface modification of orthopedic implants has made certain progress, the current coating has insufficient bonding strength, resulting in the inability to maintain biological functions for a long time. Therefore, there is an urgent need for a new method to prevent infection and promote tissue repair in clinical practice to meet the challenges of implant-related infections. Summary of the invention

[0004] In view of the problem in the prior art that the bonding strength between the coating and the substrate is insufficient, resulting in the inability to maintain the coating function for a long time, the present invention provides a polyvinyl alcohol-based composite material and a preparation method and application thereof.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0006] In a first aspect, the present invention provides a polyvinyl alcohol-based composite material, comprising a titanium alloy substrate treated by a femtosecond laser, and a gel coating containing a polyvinyl alcohol-based polymer represented by formula (I) on the titanium alloy substrate;

[0007]

[0008] The terpyridine and catechol groups of the polyvinyl alcohol-based polymer are coordinated with Cu 2+ .

[0009] Compared with the prior art, the polyvinyl alcohol-based composite material provided by the present invention adopts a titanium alloy treated by femtosecond laser as a matrix. The femtosecond laser treatment can produce a unique micro-nano multi-level structure on the surface of the titanium alloy, which can effectively increase the contact area between the gel coating and the matrix, thereby significantly enhancing the bonding strength between the gel coating and the matrix; at the same time, a polyvinyl alcohol-based polymer with a specific structure is selected as a functional coating, wherein the polymer has a high content of catechol groups, which can improve the Cu 2+ The grafting rate is 1.34%, and the terpyridine group and catechol group are connected with Cu 2+ The coordination effect of Cu 2+ Chelating and anchoring in polyvinyl alcohol polymer improves the stability of the material and realizes Cu 2+ Long-term slow release of Cu in polyvinyl alcohol polymer can achieve sustained antibacterial effect; in addition, by introducing a specific content of terpyridine and catechol groups, the Cu in polyvinyl alcohol polymer can be controlled. 2+ The content of Cu 2+ The introduction of can not only improve the biocompatibility and antibacterial properties of the material, but also avoid the cytotoxic reaction and protein adsorption induced by high concentrations of metal ions.

[0010] The present invention introduces an appropriate amount of Cu into a polyvinyl alcohol-based polymer with a specific structure. 2+ , can be obtained by Cu 2+ The slow release of Cu 2+ The introduction of can further enhance the osteogenicity of polyvinyl alcohol-based composites by regulating the synthesis of extracellular matrix and cell differentiation, and has broad application prospects in the field of bone repair implant materials.

[0011] Furthermore, the thickness of the gel coating is 15 nm to 25 nm.

[0012] Furthermore, the preparation method of the polyvinyl alcohol-based polymer comprises the following steps:

[0013] The compound represented by formula (II) and dopamine hydrochloride are subjected to an amidation reaction in a carboxyl activator and a reaction solvent to obtain a polyvinyl alcohol-based polymer represented by formula (I);

[0014]

[0015] Furthermore, in combination with the preparation method of the polyvinyl alcohol-based polymer, the carboxyl activator is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride.

[0016] Furthermore, in combination with the above-mentioned method for preparing the polyvinyl alcohol-based polymer, the reaction solvent is MES buffer.

[0017] Exemplarily, the pH of the MES buffer is 4.8, and the concentration is 0.1 mol / L.

[0018] Furthermore, in combination with the above-mentioned method for preparing the polyvinyl alcohol-based polymer, the mass ratio of the compound represented by formula (II), the carboxyl activator and dopamine hydrochloride is 5:12-14:12-14.

[0019] Preferably, the mass ratio of the compound represented by formula (II), the carboxyl activator and dopamine hydrochloride is 5:13:13.

[0020] Preferably, the concentrations of the compound represented by formula (II), the carboxyl activator and dopamine hydrochloride after being dissolved in the reaction solvent are 5-10 mg / mL, 13-26 mg / mL and 13-26 mg / mL respectively.

[0021] Furthermore, in combination with the above-mentioned method for preparing the polyvinyl alcohol-based polymer, the temperature of the amidation reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

[0022] It should be noted that after the reaction is completed, the process further includes: dialyzing the reaction solution in deionized water for 3 days and freeze-drying to obtain the polyvinyl alcohol-based polymer represented by formula (I).

[0023] The present invention introduces terpyridine groups and catechol groups into polyvinyl alcohol molecules through a simple amidation reaction, which effectively improves the antibacterial property of polyvinyl alcohol. The introduction of terpyridine groups and catechol groups can also enhance the adhesion of implants to biological cells and improve the stability of implants to bone tissue. In addition, terpyridine groups and catechol groups can also be used as active groups to participate in regulating the tissue microenvironment around the implant, promoting more effective tissue repair and regeneration. The specific content of terpyridine groups and catechol groups is also conducive to enhancing the mechanical strength and toughness of polyvinyl alcohol-based gels, making them more adaptable to the mechanical properties requirements of bone implants during use.

[0024] Furthermore, the preparation method of the compound represented by formula (II) comprises the following steps:

[0025] The compound represented by formula (III) is subjected to an amidation reaction with 2,2':6',2"-terpyridine-4'-amine in the presence of a catalyst, a base and a reaction solvent to obtain the compound represented by formula (II);

[0026]

[0027] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the catalyst is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride.

[0028] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the base is 4-dimethylaminopyridine and the reaction solvent is dimethyl sulfoxide.

[0029] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the temperature of the amidation reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

[0030] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the mass volume ratio of the compound represented by the formula (III) to the reaction solvent is 10 mg: 1 mL to 20 mg: 1 mL; the amount of the 2,2':6',2"-terpyridine-4'-amine added is 17% to 28% of the mass of the compound represented by the formula (II); the amount of the catalyst added is 17% to 28% of the mass of the compound represented by the formula (II); and the amount of the base added is 6.5% to 22% of the mass of the compound represented by the formula (II).

[0031] Furthermore, the preparation method of the compound represented by formula (II) comprises the following steps:

[0032] Polyvinyl alcohol and succinic anhydride are subjected to esterification reaction in a reaction solvent and an amine catalyst to obtain a compound represented by formula (III).

[0033] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the reaction solvent is dimethyl sulfoxide.

[0034] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the amine catalyst is triethylamine.

[0035] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the temperature of the esterification reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

[0036] Furthermore, in combination with the preparation method of the compound represented by the above formula (II), the mass volume ratio of the polyvinyl alcohol to the reaction solvent is 1.5 mg:1 mL to 2.5 mg:1 mL; the volume ratio of the reaction solvent to triethylamine is 1:80 to 1:100; and the mass concentration of the succinic anhydride after being dissolved in the reaction solvent is 0.84% ​​to 1.4%.

[0037] Specifically, the chemical reaction equation for preparing the polyvinyl alcohol-based polymer represented by formula (I) of the present invention is as follows:

[0038]

[0039]

[0040] The preparation method of the polyvinyl alcohol-based polymer provided by the invention has a simple process route and mild operating conditions, is suitable for large-scale industrial production and application, and has good economic benefits and development prospects.

[0041] In a second aspect, the present invention further provides a method for preparing a polyvinyl alcohol-based composite material, characterized in that it comprises the following steps:

[0042] S1, dissolving the polyvinyl alcohol-based polymer represented by formula (I) in water to obtain a polyvinyl alcohol-based polymer solution; and uniformly mixing the polyvinyl alcohol-based polymer solution with a MOPs buffer to obtain an impregnation solution;

[0043] S2, pre-treating the titanium alloy substrate by using a femtosecond laser, and cleaning the substrate after the treatment to obtain a pre-treated titanium alloy substrate;

[0044] S3, adding the pretreated titanium alloy substrate into the impregnation solution, soaking, drying, and then impregnating in a copper solution, drying, to obtain a polyvinyl alcohol-based composite material.

[0045] Furthermore, the concentration of the polyvinyl alcohol-based polymer solution is 2 mg / mL to 4 mg / mL.

[0046] Furthermore, the volume ratio of the polyvinyl alcohol-based polymer solution to the MOPs buffer solution is 1:1.5 to 1:2.5.

[0047] Furthermore, the MOPs buffer is Tris-MOPs-SDS electrophoresis buffer (20×, pH 8.3).

[0048] Furthermore, the processing frequency of the femtosecond laser is 610 Hz to 630 Hz, the power is 4.3 Hz to 4.4 Hz, the line spacing is 0.03 μm to 0.05 μm, and the speed is 490 femtoseconds to 510 femtoseconds.

[0049] Furthermore, the immersion time in the immersion liquid is 10 hours to 14 hours.

[0050] Furthermore, the copper solution is a copper chloride solution.

[0051] Furthermore, the concentration of the copper chloride solution is 0.2 mg / mL to 0.5 mg / mL.

[0052] Furthermore, the immersion time in the copper solution is 1 h to 1.5 h.

[0053] The present invention uses femtosecond laser technology to perform surface treatment on the titanium alloy matrix to enhance the bonding strength between the gel and the titanium alloy matrix, and introduces copper ions into a polyvinyl alcohol-based polymer with a specific structure to construct a bioactive surface that promotes bone cell adhesion and proliferation, thereby achieving stable and lasting antibacterial effects and promoting directional differentiation of bone cells. It is expected to bring more reliable and lasting therapeutic effects to the field of bone disease treatment and implant repair in clinical practice, and has broad application prospects.

[0054] In a third aspect, the present invention also provides the use of the above polyvinyl alcohol-based composite material in the preparation of orthopedic implants.

[0055] The polyvinyl alcohol-based composite material provided by the present invention has good safety and biocompatibility, has long-lasting and excellent antibacterial activity against Gram-positive bacteria, and has a good ability to promote tissue repair, is suitable for application in the preparation of orthopedic implants, and has broad application value in the field of medical biotechnology. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is the H-NMR spectrum of the PVA-TP-CA material prepared in Example 1 of the present invention;

[0057] Figure 2 XPS spectra of the PVA-TP-CA / Cu@Ti sample prepared in Example 2 of the present invention, where (a) is the full spectrum, and (b) is Cu2p;

[0058] Figure 3 SEM images of the PVA-TP-CA material prepared in Example 1 of the present invention and the PVA-TP-CA / Cu@Ti sample prepared in Example 2; wherein (a) is the PVA-TP-CA material, (b) is a local enlarged view of the portion indicated by a red circle in (a), (c) is the PVA-TP-CA / Cu@Ti sample, and (d) is a local enlarged view of the portion indicated by a red circle in (c); the upper left corners of (a) and (b) are test images of the hydrophobic contact angles of the corresponding materials;

[0059] Figure 4 A comparison chart of the bonding strength between the PVA-TP-CA coating and the titanium alloy substrate in the PVA-TP-CA / Cu@Ti samples prepared in Example 2 of the present invention and Comparative Example 1;

[0060] Figure 5 This is the cumulative release graph of copper ions of the PVA-TP-CA / Cu@Ti sample prepared in Example 2 of the present invention;

[0061] Figure 6 Comparison of the proliferation of rat bone marrow mesenchymal stem cells in PVA-TP-CA / Cu@Ti samples prepared in different copper chloride solutions;

[0062] Figure 7 The antibacterial performance comparison chart of PVA-TP-CA / Cu@Ti samples prepared in different copper chloride solutions, where (A) is the morphology of Staphylococcus aureus on the surface of different samples, (B) is the morphology of Escherichia coli on the surface of different samples, (C) is the comparison chart of the antibacterial ability of different samples against Staphylococcus aureus, and (D) is the comparison chart of the antibacterial ability of different samples against Escherichia coli. DETAILED DESCRIPTION

[0063] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0064] The polyvinyl alcohol (PVA) used in the following examples is polyvinyl alcohol 1799, manufactured by Aladdin; 2,2':6',2"-terpyridine-4'-amine (TP) is from Zhongkeshen; and dopamine hydrochloride is from McLean.

[0065] The titanium alloy substrate used in the following examples is a titanium sheet with a size of 10 mm×10 mm×1 mm. Before use, the titanium sheet was polished with 600-mesh and 1500-mesh silicon carbide sandpapers, respectively, and rinsed with deionized water.

[0066] Example 1

[0067] A method for preparing a polyvinyl alcohol-based polymer comprises the following steps:

[0068] Step a, adding 2.5 g of polyvinyl alcohol to 100 mL of dimethyl sulfoxide at 95° C., then adding 1 mL of triethylamine and 0.35 g of succinic anhydride, stirring the resulting mixture at 95° C. for 30 min, stirring at room temperature overnight, then adding the reaction solution into a dialysis bag with a molecular weight cutoff of 3.5 kDa, dialyzing with deionized water for one week, and freeze-drying to obtain PVA-COOH;

[0069] Step b, taking 1 g of the prepared PVA-COOH, 0.28 g of TP (2,2':6',2"-terpyridine-4'-amine), 0.17 g of EDCI (1-ethyl-3-(3-dimethylpropyl)carbodiimide hydrochloride) and 0.112 g of DMAP (4-dimethylaminopyridine) were added to 100 mL of dimethyl sulfoxide, stirred at 95 ° C for 30 min, stirred at room temperature overnight, and then the reaction solution was added to a dialysis bag with a molecular weight cutoff of 8.0 kDa and dialyzed with deionized water for 3 days, and freeze-dried to obtain PVA-TP-COOH;

[0070] Step c, add 0.3 g of the prepared PVA-TP-COOH, 0.78 g of EDCI, and 0.78 g of dopamine hydrochloride to 30 mL of 0.1 mol / L MES buffer at pH 4.8, mix well, stir at room temperature overnight, add the reaction solution to a dialysis bag with a molecular weight cutoff of 8.0 kDa, dialyze with deionized water for 3 days, and freeze-dry to obtain PVA-TP-CA.

[0071] The above chemical reaction equation is as follows:

[0072]

[0073]

[0074] The reaction raw materials of the above substances can also be replaced by other proportions specified in the specification of the present invention, and the reaction temperature and time can also be replaced by other conditions specified in the specification of the present invention. As long as they are within the scope specified by the present invention, PVA-TP-CA with the same structure and performance can be obtained.

[0075] Example 2

[0076] This embodiment provides a method for preparing a polyvinyl alcohol-based composite material, comprising the following steps:

[0077] S1, adding the PVA-TP-CA prepared in Example 1 to deionized water to obtain a PVA-TP-CA solution with a concentration of 3 mg / mL; mixing the PVA-TP-CA solution with the MOPs buffer solution at a volume ratio of 1:2 to obtain an impregnation solution;

[0078] S2, the titanium alloy substrate is treated by femtosecond laser technology, the frequency of the femtosecond laser is 620 Hz, the power is 4.35 Hz, the line spacing is 0.04 μm, and the speed is 500 femtoseconds. After the treatment, the titanium alloy substrate is cleaned with 75% alcohol and dried to obtain a pretreated titanium alloy substrate;

[0079] S3, adding the pretreated titanium alloy substrate to the above-mentioned impregnation solution, soaking it at room temperature for 12 hours, then drying it at room temperature, and then adding it to a 0.5 mg / mL copper chloride solution, soaking it for 1 hour, and drying it at room temperature to obtain a titanium alloy substrate with a PVA-TP-CA coating, recorded as PVA-TP-CA / Cu@Ti.

[0080] Example 3

[0081] This embodiment provides a method for preparing a polyvinyl alcohol-based composite material, comprising the following steps:

[0082] S1, adding the PVA-TP-CA prepared in Example 1 into deionized water to obtain a PVA-TP-CA solution with a concentration of 2 mg / mL; mixing the PVA-TP-CA solution with the MOPs buffer solution at a volume ratio of 1:1.5 to obtain an impregnation solution;

[0083] S2, the titanium alloy substrate is treated by femtosecond laser technology, the frequency of the femtosecond laser is 610 Hz, the power is 4.3 Hz, the line spacing is 0.03 μm, and the speed is 490 femtoseconds. After the treatment, the titanium alloy substrate is cleaned with 75% alcohol and dried to obtain a pretreated titanium alloy substrate;

[0084] S3, adding the pretreated titanium alloy substrate to the above-mentioned impregnation solution, soaking it at room temperature for 14 hours, then drying it at room temperature, and then adding it to a 0.2 mg / mL copper chloride solution, soaking it for 1.5 hours, and drying it at room temperature to obtain a titanium alloy substrate with a PVA-TP-CA coating, recorded as PVA-TP-CA / Cu@Ti.

[0085] Example 4

[0086] This embodiment provides a method for preparing a polyvinyl alcohol-based composite material, comprising the following steps:

[0087] S1, adding the PVA-TP-CA prepared in Example 1 into deionized water to obtain a PVA-TP-CA solution with a concentration of 4 mg / mL; mixing the PVA-TP-CA solution with the MOPs buffer solution at a volume ratio of 1:2.5 to obtain an impregnation solution;

[0088] S2, the titanium alloy substrate is treated by femtosecond laser technology, the frequency of the femtosecond laser is 630 Hz, the power is 4.4 Hz, the line spacing is 0.05 μm, and the speed is 510 femtoseconds. After the treatment, the titanium alloy substrate is cleaned with 75% alcohol and dried to obtain a pretreated titanium alloy substrate;

[0089] S3, adding the pretreated titanium alloy substrate to the above-mentioned impregnation solution, soaking it at room temperature for 10 hours, then drying it at room temperature, and then adding it to a 0.5 mg / mL copper chloride solution, soaking it for 1 hour, and drying it at room temperature to obtain a titanium alloy substrate with a PVA-TP-CA coating, recorded as PVA-TP-CA / Cu@Ti.

[0090] Comparative Example 1

[0091] This comparative example provides a method for preparing a polyvinyl alcohol-based composite material. The only difference from Example 2 is that the step of performing femtosecond laser treatment on the titanium alloy substrate is omitted. The specific steps are as follows:

[0092] S1, adding the PVA-TP-CA prepared in Example 1 to deionized water to obtain a PVA-TP-CA solution with a concentration of 3 mg / mL; mixing the PVA-TP-CA solution with the MOPs buffer solution at a volume ratio of 1:2 to obtain an impregnation solution;

[0093] S2, adding the titanium alloy substrate to the above-mentioned impregnation solution, soaking it at room temperature for 12 hours, then drying it at room temperature, and then adding it to a 0.5 mg / mL copper chloride solution, soaking it for 1 hour, and drying it at room temperature to obtain a titanium alloy substrate with a PVA-TP-CA coating.

[0094] Characterization

[0095] Figure 1 This is the H NMR spectrum of the PVA-TP-CA material prepared in Example 1. As can be seen from the figure, the chemical shift of the TP group is mainly concentrated between 7.0ppm and 9.0ppm, and the chemical shift of the CA group is mainly concentrated between 6.0ppm and 7.0ppm, indicating that TP and CA are successfully grafted onto the polyvinyl alcohol molecular chain.

[0096] The XPS graph of PVA-TP-CA / Cu@Ti prepared in Example 2 is as follows: Figure 2 As shown. Figure 2 As can be seen in (a), the binding energy of Cu2p in the PVA-TP-CA / Cu coating is 932.6 eV. Figure 2 As can be seen in (b), in the 2P orbital of copper, the satellite peaks of copper ions are mainly located at 943eV and 961eV, proving that copper ions are grafted into the coating.

[0097] The SEM images of the PVA-TP-CA material prepared in Example 1 and the PVA-TP-CA / Cu@Ti prepared in Example 2 are shown in FIG. Figure 3 As shown in the figure, it can be seen that the grafting of copper ions increases the roughness of the copper alloy substrate. And many well-known titanium alloys have poor hydrophilicity. Figure 3 (a) and Figure 3 (b) The contact angle test in the upper left corner shows that the introduction of the coating on the titanium alloy substrate significantly improves the hydrophilicity of the substrate, and the hydrophilicity is also improved to a certain extent after grafting copper ions, which is beneficial to promote cell adhesion, improve the bonding strength between the implant and the surrounding bone tissue, and accelerate the bone healing process.

[0098] Performance Testing

[0099] 1. Bonding strength

[0100] The bonding strength test of the coating is carried out by glue pulling method. According to ISO13779.2, 3M DP460 glue with high bonding strength and two titanium rods with a diameter of 1mm and a length of 5cm are selected. The titanium rod with double-sided coating is glued between the cross sections of the two titanium rods using 3M DP460, and stretched using a mechanical testing machine at a stretching rate of 1mm / min.

[0101] The test results of the titanium alloy substrate with PVA-TP-CA coating prepared in Example 2 and Comparative Example 1 are as follows: Figure 4 shown.

[0102] It can be seen from the figure that the bonding strength between the PVA-TP-CA coating and the titanium alloy substrate in the sample prepared in Example 2 is 29.04 MPa, while the bonding strength between the PVA-TP-CA coating and the titanium alloy substrate in the sample prepared in Comparative Example 1 is 38.8 MPa. This proves that the bonding strength between the titanium alloy substrate and the PVA-TP-CA coating is significantly enhanced after being treated by femtosecond laser.

[0103] 2. Release of copper ions

[0104] The PVA-TP-CA / Cu@Ti (10mm×10mm×1mm) sample prepared in Example 2 was immersed in 5mL of phosphate buffer at pH=7.4. Three parallel groups were set up. Samples were taken at 1d, 2d, 3d, 6d, 7d, 8d, 9d, and 12d to detect the copper ion concentration, and the buffer was replaced with fresh PBS. The copper ion concentration was detected by inductively coupled plasma optical emission spectrometry (ICP-MS). The results are shown in Table 1 and Figure 5 described.

[0105] Table 1 Copper ion release

[0106] Release amount (ppb) RSD / % of three groups of samples 1d 13.534 3.11 2d 27.143 2.114 3d 36.133 4.543 6d 36.244 2.311 7d 39.381 3.243 8d 48.948 8.261 9d 50.108 8.978 12d 62.293 5.768

[0107] This indicates that the PVA-TP-CA / Cu@Ti sample prepared in the embodiment of the present invention can realize the slow release of copper ions, thereby achieving the effects of lasting antibacterial and promoting tissue repair.

[0108] 3. Promote cell proliferation

[0109] The PVA-TP-CA prepared in Example 1 was immersed in copper chloride solutions of different concentrations, and the concentrations of the copper chloride solutions were set to 0.1 mg / mL, 0.2 mg / mL, 0.5 mg / mL and 1 mg / mL, respectively. The PVA-TP-CA / Cu@Ti sample was prepared in the same manner as in Example 2.

[0110] The prepared samples were placed in 24-well plates, and rat bone marrow mesenchymal stem cells (BMSCs) were inoculated on the coating surface of each group of samples. The number of cells inoculated in each well was 1.5×10 4 , placed in a 37℃ cell culture incubator for 1d and 3d respectively. After the culture, the samples were transferred to a new 24-well plate and gently rinsed with PBS buffer for 3 times, 5min each time. CCK-8 and complete culture medium were mixed evenly in a volume ratio of 1:9. 1mL of the mixed solution was added to each well, shaken, and incubated in a 37℃ cell culture incubator in the dark for 2.5h. 100μL of the reaction solution was taken into a 96-well plate, and the absorbance value of each group of sample solutions was detected by an enzyme marker at a detection wavelength of 450nm. The results are shown in Table 2 and Figure 6 shown.

[0111] Table 2 Cell proliferation of rat bone marrow mesenchymal stem cells and PVA-TP-CA / Cu@Ti samples prepared with different concentrations of copper chloride solution

[0112]

[0113] 4. Antibacterial properties

[0114] The PVA-TP-CA / Cu@Ti samples prepared from the above copper chloride solutions of different concentrations were placed in a 24-well plate with the coating facing upward. 1 mL of 1×10 8 CFU / mL of Staphylococcus aureus and a concentration of 1×10 6 CFU / mL of Escherichia coli were added to the surface of each group of samples, and the culture plates were placed in a 37℃ constant temperature incubator for 24 hours. The bacterial suspension in each well was collected, and the antibacterial rate of each group of samples was detected and calculated by multiple dilution method and plate coating counting method; 100μL of the bacterial suspension after multiple gradient dilution was evenly coated on the agar plate, and placed in a 37℃ constant temperature incubator for 24 hours; after taking out the plate, the plate with a colony count between 30 and 300 was selected, the number of colonies grown on the plate was calculated, and then the number of live bacteria in the culture solution around the sample was calculated according to the dilution multiple. The results are as follows Figure 7 And as shown in Table 3.

[0115] Table 3 Performance of PVA-TP-CA / Cu@Ti samples against Staphylococcus aureus and Escherichia coli

[0116]

[0117] It can be seen that the PVA-TP-CA / Cu@Ti sample prepared in the embodiment of the present invention has excellent anti-Staphylococcus aureus and Escherichia coli effects. Considering the cell proliferation effect and antibacterial effect, the PVA-TP-CA / Cu@Ti sample prepared in 0.5 mg / mL copper chloride solution has the best performance.

[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A polyvinyl alcohol-based composite material, characterized in that: It comprises a titanium alloy substrate treated by a femtosecond laser, and a gel coating containing a polyvinyl alcohol-based polymer represented by formula (I) on the titanium alloy substrate; The terpyridine and catechol groups of the polyvinyl alcohol-based polymer are coordinated with Cu 2+ .

2. The polyvinyl alcohol-based composite material according to claim 1, characterized in that: The thickness of the gel coating is 15nm-25nm.

3. The polyvinyl alcohol-based composite material according to claim 1, characterized in that: The preparation method of the polyvinyl alcohol-based polymer comprises the following steps: The compound represented by formula (II) and dopamine hydrochloride are subjected to an amidation reaction in a carboxyl activator and a reaction solvent to obtain a polyvinyl alcohol-based polymer represented by formula (I); 4. The polyvinyl alcohol-based composite material according to claim 3, characterized in that: The carboxyl activator is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride; and / or The reaction solvent is MES buffer; and / or The mass ratio of the compound represented by formula (II), the carboxyl activator and dopamine hydrochloride is 5:12-14:12-14; and / or The temperature of the amidation reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

5. The polyvinyl alcohol-based composite material according to claim 3 or 4, characterized in that: The preparation method of the compound represented by formula (II) comprises the following steps: The compound represented by formula (III) is subjected to an amidation reaction with 2,2':6',2"-terpyridine-4'-amine in the presence of a catalyst, a base and a reaction solvent to obtain the compound represented by formula (II); 6. The polyvinyl alcohol-based composite material according to claim 5, characterized in that: The catalyst is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride; and / or The base is 4-dimethylaminopyridine; and / or The reaction solvent is dimethyl sulfoxide; and / or The temperature of the amidation reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

7. The polyvinyl alcohol-based composite material according to claim 5, characterized in that: The preparation method of the compound represented by formula (II) comprises the following steps: Polyvinyl alcohol and succinic anhydride are subjected to esterification reaction in a reaction solvent and an amine catalyst to obtain a compound represented by formula (III).

8. The polyvinyl alcohol-based composite material according to claim 7, characterized in that: The reaction solvent is dimethyl sulfoxide; and / or The amine catalyst is triethylamine; and / or The temperature of the esterification reaction is 20° C. to 30° C., and the reaction time is 8 h to 12 h.

9. The method for preparing the polyvinyl alcohol-based composite material according to any one of claims 1 to 8, characterized in that: The steps include: S1, dissolving the polyvinyl alcohol-based polymer represented by formula (I) in water to obtain a polyvinyl alcohol-based polymer solution; and uniformly mixing the polyvinyl alcohol-based polymer solution with a MOPs buffer to obtain an impregnation solution; S2, pre-treating the titanium alloy substrate by using a femtosecond laser, and after the treatment, cleaning to obtain a pre-treated titanium alloy substrate; S3, adding the pretreated titanium alloy substrate into the impregnation solution, soaking, drying, and then impregnating in a copper solution, drying, to obtain a polyvinyl alcohol-based composite material.

10. Use of the polyvinyl alcohol-based composite material according to any one of claims 1 to 8 in the preparation of orthopedic implants.

Citation Information

Patent Citations

  • Wound dressing membrane

    CA1305055C

  • Antibacterial collagen-based bone repair material

    CN110898258A

  • Antibacterial polymer polyvinyl alcohol material and method and application thereof

    CN111718435A

  • Construction method of titanium alloy surface composite hydrogel coating capable of reducing bone tissue abrasion

    CN113384750A

  • Preparation and application of composite hydrogel capable of releasing nitric oxide through light control

    CN114129780A