Black phosphorus preparation device and method for preparing black phosphorus by using same
The black phosphorus preparation device transmitted through gradient heating uses continuous operations of high-temperature chambers, rotary vaporization chambers and low-temperature chambers to solve the problem of low black phosphorus production efficiency in the prior art, and achieves efficient and suitable industrial black phosphorus preparation. Yield and yield increased significantly.
Patent Information
- Application Number
- CN202411197942.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing black phosphorus preparation methods have problems such as low production efficiency, high equipment requirements, large safety hazards and small output, which limit their industrial promotion.
The black phosphorus preparation device using gradient heating transmission, including a high-temperature room, a rotary vaporization room and a low-temperature room, improves the utilization rate of equipment through continuous operation, uses a rotary furnace to react, and improves the production efficiency of black phosphorus.
It has achieved efficient preparation of black phosphorus, improved production efficiency, is suitable for industrial promotion, has significantly increased output, and a yield of more than 96.82%.
Smart Images

Figure CN119075835A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor materials, and in particular relates to a black phosphorus preparation device and a method for preparing black phosphorus using the device. Background Art
[0002] Black phosphorus is a new type of two-dimensional semiconductor material that has received widespread attention in recent years. Compared with graphene, black phosphorus not only has a two-dimensional layered structure and higher carrier mobility, but also has a natural band gap in its structure. By adjusting the number of layers, it can achieve the conversion between the insulating and conductive states, which is not available in graphene. Therefore, black phosphorus has broad application prospects in biomedicine, electronic thin films, optoelectronic technology, catalysis and other fields.
[0003] The preparation method of black phosphorus has been studied since 1914. It is mainly divided into two categories: pressure method and catalytic method. The subdivisions include high-pressure method, ball milling method, mercury catalytic method, bismuth melting method, mineralization method and chemical vapor deposition method. Among them, the high-pressure method and ball milling method belong to the pressure method. The preparation process requires relatively harsh high pressure, high requirements for equipment, and major safety hazards, which are not conducive to industrial production; the mercury catalytic method is too toxic, which limits its use; the bismuth melting method will introduce impurities; the mineralization method has a small output of black phosphorus due to its equipment requirements, and it is difficult to apply on a large scale; the chemical vapor deposition method also has a small output of black phosphorus due to its equipment requirements, and the production temperature is too high. In addition, the wet chemical method used to make black phosphorus nanosheets also has yield problems.
[0004] By analyzing the above methods and existing problems, it is generally believed that although the mineralization method has a low yield in the existing technology, its preparation conditions are mild and the product crystallinity is good, which is more promising for industrialization. In this regard, researchers have also conducted relevant technical research. For example, patent CN112939065A discloses a method for preparing a black phosphorus catalyst. This method mixes tin triphosphide and tin iodide compounds and then performs a programmed temperature treatment under an inert atmosphere or vacuum to obtain an efficient catalyst for preparing black phosphorus by the mineralization method.
[0005] Patent CN106087050A discloses a method for preparing black phosphorus single crystals at low pressure, in which raw materials red phosphorus, catalyst tin and mineralizer high tin iodide are placed in a quartz tube, vacuum sealed, and heated and cooled in a muffle furnace to obtain black phosphorus crystals. Patent CN110878425A discloses a method for rapidly preparing high-quality two-dimensional black phosphorus crystals by seed induction, in which black phosphorus seed crystals are weighed and placed in the cold end of a quartz tube under an inert atmosphere, and a porous gasket is used to isolate the middle, raw materials red phosphorus, catalyst tin and transport agent high tin iodide are weighed and placed in a quartz tube, vacuum sealed, and the quartz tube is heated by optimized program heating and cooling to obtain high-purity, high-quality two-dimensional black phosphorus crystals. Patent CN115449898A discloses a method for preparing black phosphorus. In this method, under an inert atmosphere, the raw material red phosphorus and the transport agent high tin iodide are weighed and placed in the high-temperature end of a closed reactor, and monoclinic phosphorus crystals are obtained by temperature control. Catalyst tin is weighed and placed in the high-temperature end to continue the temperature control reaction, and finally high-quality black phosphorus crystals are obtained at the low-temperature end of the closed reactor.
[0006] The above method is aimed at optimizing the mineralization method, focusing on the preparation and use of catalysts and temperature control. The reaction uses a vacuum-sealed reactor, such as a quartz tube, which limits the total amount of black phosphorus prepared in a single time and is not conducive to large-scale industrial promotion. Summary of the invention
[0007] In view of the problem of low black phosphorus production efficiency in the prior art, the present invention provides a black phosphorus preparation device and a method for preparing black phosphorus using the device. The reaction is carried out by gradient temperature transmission, and continuous operation can be performed. By improving the utilization rate of the equipment, the black phosphorus production efficiency is improved, which is conducive to industrial promotion.
[0008] The present invention is achieved through the following technical solutions: A black phosphorus preparation device, comprising a high-temperature chamber, a high-temperature rotary vaporization chamber and a low-temperature chamber connected in series; The high temperature chamber comprises a high temperature chamber I, a high temperature chamber II and a high temperature chamber III which are connected in series in sequence.
[0009] Furthermore, the high temperature chamber I is connected to the feed chamber, and there are two chambers in the feed chamber; the high temperature rotary vaporization chamber and the low temperature chamber are a group, and multiple groups are connected in parallel.
[0010] Furthermore, the high temperature chamber I, high temperature chamber II, high temperature chamber III, high temperature rotary vaporization chamber and low temperature chamber independently control the temperature.
[0011] Furthermore, the high temperature chambers I, II and III are provided with spiral lifting plates to transfer materials by rotation; the inner wall of the high temperature rotary vaporization chamber is a honeycomb structure, the side length of the honeycomb is 0.1~0.5cm, and the depth of the honeycomb is equal to the side length of the honeycomb.
[0012] In the present invention, the method for preparing black phosphorus by the device comprises the following steps: (1) uniformly mixing red phosphorus and catalyst A to prepare a raw material; (2) The prepared raw material in step (1) is added to a high temperature chamber, and is subjected to a gradient temperature treatment in high temperature chamber I, high temperature chamber II and high temperature chamber III in sequence, and then enriched in a high temperature rotary vaporization chamber to which a catalyst has been added in advance, and then subjected to a heat preservation treatment for 6 to 8 hours; (3) After heat preservation treatment in the high-temperature rotary vaporization chamber in step (2), the material is transferred to a low-temperature chamber for cooling treatment, and black phosphorus is obtained after purification treatment.
[0013] Furthermore, the catalyst A is a mixture of tin tetraiodide and iodine in a mass ratio of 1 to 5:1; the catalyst B is tin; the mass ratio of the catalyst A to red phosphorus is 1 to 2:10; the amount of the catalyst B added is 0.01 to 0.05V, in g, V is the volume of the high-temperature rotary gasification chamber, in cm 3 .
[0014] Furthermore, the temperatures in the high temperature chamber I, high temperature chamber II and high temperature chamber III are 250~260°C, 300~310°C and 350~360°C respectively; the temperature of the high temperature rotary vaporization chamber is 510±10°C.
[0015] Furthermore, the temperature of the cryogenic chamber is 400±10°C, and after enriching the material for 4 hours, the valve is closed for cooling treatment. After the temperature drops to 300±5°C, purification treatment is carried out; the purification treatment method is to purge the bottom of the cryogenic chamber with normal temperature nitrogen, wait for the black phosphorus to drop to 200±5°C, vacuum dry and cool to 100±5°C in a nitrogen atmosphere, turn off the vacuum drying, and naturally cool to room temperature.
[0016] Furthermore, the retention time of the prepared raw materials in high temperature chambers I, II and III is 2 to 3 hours, and the enrichment time in the high temperature rotary gasification chamber is twice the retention time of the prepared raw materials in the high temperature chambers.
[0017] Furthermore, the red phosphorus particle size D50 in step (1) is ≤30 μm; the feeding rate of the prepared raw material in step (2) is 0.1 MC, in g / min, and M is the cross-sectional area of the high temperature chamber, in cm 2 , C is the transmission rate in the high temperature chamber, unit is cm / min. Beneficial Effects
[0018] The preparation method of black phosphorus provided by the present invention uses a rotary furnace as a main reaction equipment, and performs reaction by gradient temperature transmission, which can be operated continuously, improves the utilization rate of equipment, improves the production efficiency of black phosphorus, and is conducive to industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a schematic diagram of a black phosphorus preparation device of the present invention; Figure 2 The X-ray diffraction spectrum of the black phosphorus crystal prepared in Example 1; Figure 3 This is a scanning electron microscope image of the black phosphorus crystal prepared in Example 1. DETAILED DESCRIPTION
[0020] The present invention is described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited by the embodiments. All technologies implemented based on the above content of the present invention are included in the scope of protection intended by the present invention.
[0021] The schematic diagram of the black phosphorus preparation device of the present invention is as follows Figure 1 As shown, the black phosphorus preparation device comprises a feed chamber, a high temperature chamber, a high temperature rotary vaporization chamber and a low temperature chamber connected in series in sequence; the high temperature chamber comprises a high temperature chamber I, a high temperature chamber II and a high temperature chamber III connected in series in sequence; there are two chambers in the feed chamber, namely, feed chamber ① and feed chamber ②, each chamber has an independent feed port, and the two chambers share a discharge port controlled by a valve; the high temperature rotary vaporization chamber and the low temperature chamber are a group, and the two groups are connected in parallel, namely, high temperature rotary vaporization chamber ①, high temperature rotary vaporization chamber ②, low temperature chamber ① and low temperature chamber ②; the high temperature chamber I, high temperature chamber II, high temperature chamber III, high temperature rotary vaporization chamber and low temperature chamber independently control the temperature; The high temperature chamber I, high temperature chamber II and high temperature chamber III are equipped with spiral lifting plates to transfer materials by rotation; the inner wall of the high temperature rotary vaporization chamber is a honeycomb structure with a honeycomb side length of 0.1~0.5cm, and the honeycomb depth is equal to the honeycomb side length. The cross-sectional inner diameter of the high temperature chamber is 10cm and the length is 4m; the cross-sectional inner diameter of the high temperature rotary vaporization chamber is 60cm, the length is 50cm, and the inner wall honeycomb side length is 0.5cm; the cross-sectional inner diameter of the low temperature chamber is 60cm and the length is 1m In the present invention, the red phosphorus is amorphous red phosphorus; tin, tin tetraiodide and iodine are all analytically pure; under nitrogen protection, the amorphous red phosphorus is ground to D50=24.3 by a ball mill to serve as a raw material; tin tetraiodide and iodine are mixed uniformly at a mass ratio of 3:1 to obtain catalyst A.
[0022] The method for preparing black phosphorus is now described with reference to the accompanying drawings and specific examples. Example 1
[0023] (1) Red phosphorus and catalyst A are mixed evenly in a mass ratio of 10:1 to prepare raw materials, and added into feed chamber ① and feed chamber ②. The nitrogen pipeline is opened to replace all the air in the high-temperature calcination rotary furnace with nitrogen. The replacement is stopped when the nitrogen content at both ends of the detection equipment is ≥99.5%; (2) The prepared raw materials in the feed chamber ① are pumped into the 250℃ high temperature chamber Ⅰ at a rate of 26.2g / min, and the transfer rate is 3.33cm / min. After 2h, they are transferred to the 300℃ high temperature chamber Ⅱ, and after 2h, they are transferred to the 350℃ high temperature chamber Ⅲ, and after another 2h, they are transferred into the high temperature rotary gasification chamber ① preheated to 350℃ (1413g of catalyst B tin is pre-added to both the high temperature rotary gasification chambers ① and ②). After the high temperature rotary gasification chamber ① collects materials for 4h, the materials in the 350℃ high temperature chamber begin to be transferred into the high temperature rotary gasification chamber ② through valve control. The operation of the high temperature rotary gasification chamber ① is repeated to raise the temperature in the high temperature rotary gasification chamber ① to 510±10℃, and the temperature is kept for 6h. (3) Open the valve of low-temperature chamber ①, and the material in high-temperature rotary gasification chamber ① enters the preheated 400±10℃ low-temperature chamber ①. After the low-temperature chamber ① enriches black phosphorus for 4 hours, close the valve and turn off the heat source to cool down. After 2 hours, the low-temperature chamber ① is cooled to 300±5℃ and the nitrogen gas is passed through the nitrogen pipeline at 0.28m 3 / min nitrogen is introduced to purge the bottom of low temperature chamber ①, and the temperature is lowered to 200±5℃ after 30min. The nitrogen valve is closed, and the vacuum pump is connected. The temperature is lowered to 100±5℃ under negative pressure at a vacuum degree of -90KPa. The negative pressure is stopped, and the product black phosphorus is obtained after low temperature chamber ① is cooled to room temperature. The high temperature rotary gasification chamber ② and low temperature chamber ② are operated in the same way and used alternately; The reaction product was collected for 48 hours to obtain 38742.1 g of black phosphorus crystals, with a yield of 96.82% and a production efficiency of 807.13 g / h. Its X-ray diffraction spectrum and scanning electron microscope images are shown as follows: Figure 2 and Figure 3 As shown by Figure 2 and Figure 3 It can be seen that the product is black phosphorus, which has an obvious lamellar crystal structure. Example 2
[0024] (1) Red phosphorus and catalyst A are mixed evenly in a mass ratio of 10:1 to prepare raw materials, and added into feed chamber ① and feed chamber ②. The nitrogen pipeline is opened to replace all the air in the high-temperature calcination rotary furnace with nitrogen. The replacement is stopped when the nitrogen content at both ends of the detection equipment is ≥99.5%; (2) The prepared raw materials in the feed chamber ① are pumped into the 250℃ high temperature chamber Ⅰ at a rate of 17.4g / min, and the transfer rate is 2.22cm / min. After 3h, they are transferred to the 300℃ high temperature chamber Ⅱ, and after 3h, they are transferred to the 350℃ high temperature chamber Ⅲ, and after another 3h, they are transferred into the high temperature rotary gasification chamber ① preheated to 350℃ (2826g of catalyst B tin is pre-added to both the high temperature rotary gasification chambers ① and ②). After the high temperature rotary gasification chamber ① collects materials for 6h, the materials in the 350℃ high temperature chamber begin to be transferred into the high temperature rotary gasification chamber ② through valve control. The operation of the high temperature rotary gasification chamber ① is repeated to raise the temperature in the high temperature rotary gasification chamber ① to 510±10℃ and keep warm for 8h. (3) Open the valve of low-temperature chamber ①, and the material in high-temperature rotary gasification chamber ① enters the preheated 400±10℃ low-temperature chamber ①. After the low-temperature chamber ① enriches black phosphorus for 4 hours, close the valve and turn off the heat source to cool down. After 2 hours, the low-temperature chamber ① is cooled to 300±5℃ and the nitrogen gas is passed through the nitrogen pipeline at 0.28m 3 / min nitrogen is introduced to purge the bottom of low temperature chamber ①, and the temperature is lowered to 200±5℃ after 30min. The nitrogen valve is closed, and the vacuum pump is connected. The temperature is lowered to 100±5℃ under negative pressure at a vacuum degree of -80KPa, and the negative pressure is stopped. The product black phosphorus is obtained when low temperature chamber ① is cooled to room temperature. The high temperature rotary gasification chamber ② and low temperature chamber ② are operated in the same way and used alternately; The reaction product was collected after 48 hours, and 22297.5 g of black phosphorus crystals were obtained, with a yield of 97.89% and a production efficiency of 464.53 g / h. Example 3
[0025] (1) Red phosphorus and catalyst A are mixed evenly in a mass ratio of 5:1 to prepare raw materials, and added into feed chamber ① and feed chamber ②. The nitrogen pipeline is opened to replace all the air in the high-temperature calcination rotary furnace with nitrogen. The replacement is stopped when the nitrogen content at both ends of the detection equipment is ≥99.5%; (2) The prepared raw materials in the feed chamber ① are pumped into the 250℃ high temperature chamber Ⅰ at a rate of 26.2g / min, and the transfer rate is 3.33cm / min. After 2h, they are transferred to the 300℃ high temperature chamber Ⅱ, and after 2h, they are transferred to the 350℃ high temperature chamber Ⅲ, and after another 2h, they are transferred into the high temperature rotary gasification chamber ① preheated to 350℃ (1413g of catalyst B tin is pre-added to both the high temperature rotary gasification chambers ① and ②). After the high temperature rotary gasification chamber ① collects materials for 4h, the materials in the 350℃ high temperature chamber begin to be transferred into the high temperature rotary gasification chamber ② through valve control. The operation of the high temperature rotary gasification chamber ① is repeated to raise the temperature in the high temperature rotary gasification chamber ① to 510±10℃, and the temperature is kept for 6h. (3) Open the valve of low-temperature chamber ①, and the material in high-temperature rotary gasification chamber ① enters the preheated 400±10℃ low-temperature chamber ①. After the low-temperature chamber ① enriches black phosphorus for 4 hours, close the valve and turn off the heat source to cool down. After 2 hours, the low-temperature chamber ① is cooled to 300±5℃ and the nitrogen gas is passed through the nitrogen pipeline at 0.28m 3 / min nitrogen is introduced to purge the bottom of low temperature chamber ①, and the temperature is lowered to 200±5℃ after 30min. The nitrogen valve is closed, and the vacuum pump is connected. The temperature is lowered to 100±5℃ under negative pressure at a vacuum degree of -90KPa. The negative pressure is stopped, and the product black phosphorus is obtained after low temperature chamber ① is cooled to room temperature. The high temperature rotary gasification chamber ② and low temperature chamber ② are operated in the same way and used alternately; The reaction product was collected after 48 hours, and 38898.1 g of black phosphorus crystals were obtained, with a yield of 97.21% and a production efficiency of 810.38 g / h. Example 4
[0026] (1) Red phosphorus and catalyst A are mixed evenly in a mass ratio of 5:1 to prepare raw materials, and added into feed chamber ① and feed chamber ②. The nitrogen pipeline is opened to replace all the air in the high-temperature calcination rotary furnace with nitrogen. The replacement is stopped when the nitrogen content at both ends of the detection equipment is ≥99.5%; (2) The prepared raw materials in the feed chamber ① are pumped into the 250℃ high temperature chamber Ⅰ at a rate of 17.4g / min, and the transfer rate is 2.22cm / min. After 3h, they are transferred to the 300℃ high temperature chamber Ⅱ, and after 3h, they are transferred to the 350℃ high temperature chamber Ⅲ, and after another 3h, they are transferred into the high temperature rotary gasification chamber ① preheated to 350℃ (2826g of catalyst B tin is pre-added to both the high temperature rotary gasification chambers ① and ②). After the high temperature rotary gasification chamber ① collects materials for 6h, the materials in the 350℃ high temperature chamber begin to be transferred into the high temperature rotary gasification chamber ② through valve control. The operation of the high temperature rotary gasification chamber ① is repeated to raise the temperature in the high temperature rotary gasification chamber ① to 510±10℃ and keep it warm for 6h. (3) Open the valve of low-temperature chamber ①, and the material in high-temperature rotary gasification chamber ① enters the preheated 400±10℃ low-temperature chamber ①. After the low-temperature chamber ① enriches black phosphorus for 4 hours, close the valve and turn off the heat source to cool down. After 2 hours, the low-temperature chamber ① is cooled to 300±5℃ and the nitrogen gas is passed through the nitrogen pipeline at 0.28m 3 / min nitrogen is introduced to purge the bottom of low temperature chamber ①, and the temperature is lowered to 200±5℃ after 30min. The nitrogen valve is closed, and the vacuum pump is connected. The temperature is lowered to 100±5℃ under negative pressure at a vacuum degree of -80KPa, and the negative pressure is stopped. The product black phosphorus is obtained when low temperature chamber ① is cooled to room temperature. The high temperature rotary gasification chamber ② and low temperature chamber ② are operated in the same way and used alternately; The reaction product was collected after 48 hours, and 22345.4 g of black phosphorus crystals were obtained, with a yield of 98.10% and a production efficiency of 465.53 g / h. Comparative Example 1
[0027] Comparative Example 1: A reactor with an inner diameter of 10 cm and a length of 135 cm was used to replace the reaction device in Example 1. The left end of the reactor was the raw material end, and the right end was the nucleation end. The volume of the 40 reactors was equivalent to the sum of the volume pairs of the high-temperature rotary gasification chamber and the low-temperature chamber used in Example 1. The specific steps for preparing black phosphorus are: (1) Under argon atmosphere, 160 g of amorphous red phosphorus and 1.28 g of iodine were weighed and placed at the raw material end of a closed reactor. Under room temperature, the temperature of the raw material end was raised to 300°C over 0.6 h, kept at this temperature for 9 h, and then dropped to room temperature over 1.5 h; the temperature of the nucleation end was raised to 330°C over 0.6 h, kept at this temperature for 9 h, and then dropped to room temperature over 1.5 h; the temperature control procedures of the raw material end and the nucleation end were carried out synchronously, and the temperature of the nucleation end was always 30°C higher than that of the raw material end, to obtain monoclinic phosphorus crystals; (2) The obtained monoclinic phosphorus crystals were placed in an inert atmosphere, and 2.4 g of tin was weighed and placed at the raw material end of the closed reactor. Under room temperature conditions, the temperature of the raw material end was raised to 465°C over 0.8 h, kept warm for 9 h, and then dropped to room temperature over 3 h; the temperature of the nucleation end was raised to 450°C over 0.8 h, kept warm for 9 h, and then dropped to room temperature over 3 h. The temperature control procedures of the raw material end and the nucleation end were carried out synchronously, and the temperature of the raw material end was always 15°C higher than the temperature of the nucleation end; (3) After the reaction is completed, high-quality black phosphorus crystals are finally prepared at the nucleation end.
[0028] The reaction product was collected after 48 hours, and 315.4 g of black phosphorus crystals were obtained, with a yield of 98.16%; 40 reactors were expected to produce 12,616 g of black phosphorus crystals, with a production efficiency of 262.83 g / h.
[0029] From the comparison between the embodiments and the comparative examples, it can be seen that the present invention replaces the traditional intermittent production method with a continuous feeding and continuous preparation method, which greatly improves the equipment utilization rate, thereby improving the production efficiency of black phosphorus per unit time and increasing the output of black phosphorus.
[0030] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A black phosphorus preparation device, characterized in that: The black phosphorus preparation device comprises a high temperature chamber, a high temperature rotary vaporization chamber and a low temperature chamber connected in series in sequence; The high temperature chamber comprises a high temperature chamber I, a high temperature chamber II and a high temperature chamber III which are connected in series in sequence.
2. The black phosphorus preparation device according to claim 1, characterized in that: The high temperature chamber I is connected to the feed chamber, and there are two chambers in the feed chamber; the high temperature rotary vaporization chamber and the low temperature chamber form a group, and multiple groups are connected in parallel.
3. The black phosphorus preparation device according to claim 1, characterized in that: The high temperature chamber I, high temperature chamber II, high temperature chamber III, high temperature rotary vaporization chamber and low temperature chamber control the temperature independently.
4. The black phosphorus preparation device according to claim 1, characterized in that: The high temperature chambers I, II and III are provided with spiral lifting plates to transfer materials by rotation; the inner wall of the high temperature rotary vaporization chamber is a honeycomb structure, the side length of the honeycomb is 0.1-0.5 cm, and the depth of the honeycomb is equal to the side length of the honeycomb.
5. A method for preparing black phosphorus using the device according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) uniformly mixing red phosphorus and catalyst A to prepare a raw material; (2) The prepared raw material in step (1) is added to a high temperature chamber, and is subjected to a gradient temperature treatment in high temperature chamber I, high temperature chamber II and high temperature chamber III in sequence, and then enriched in a high temperature rotary vaporization chamber to which a catalyst has been added in advance, and then subjected to a heat preservation treatment for 6 to 8 hours; (3) After heat preservation treatment in the high-temperature rotary vaporization chamber in step (2), the material is transferred to a low-temperature chamber for cooling treatment, and black phosphorus is obtained after purification treatment.
6. The method for preparing black phosphorus according to claim 5, characterized in that: The catalyst A is a mixture of tin tetraiodide and iodine in a mass ratio of 1 to 5:1; the catalyst B is tin; the mass ratio of the catalyst A to red phosphorus is 1 to 2:10; the amount of the catalyst B added is 0.01 to 0.05V, in g, V is the volume of the high-temperature rotary gasification chamber, in cm 3 .
7. The method for preparing black phosphorus according to claim 5, characterized in that: The temperatures in the high temperature chamber I, high temperature chamber II and high temperature chamber III are 250-260°C, 300-310°C and 350-360°C respectively; the temperature in the high temperature rotary vaporization chamber is 510±10°C.
8. The method for preparing black phosphorus according to claim 5, characterized in that: The temperature of the cryogenic chamber is 400±10°C. After enriching the material for 4 hours, the valve is closed for cooling treatment. After the temperature drops to 300±5°C, purification treatment is carried out. The purification method is to purge the bottom of the cryogenic chamber with normal temperature nitrogen, wait for the black phosphorus to drop to 200±5°C, vacuum dry and cool to 100±5°C in a nitrogen atmosphere, close the vacuum dryer, and cool naturally to room temperature.
9. The method for preparing black phosphorus according to claim 5, characterized in that: The retention time of the prepared raw materials in high temperature chambers I, II and III is 2 to 3 hours, and the enrichment time in the high temperature rotary gasification chamber is twice the retention time of the prepared raw materials in the high temperature chamber.
10. The method for preparing black phosphorus according to claim 5, characterized in that: The red phosphorus particle size D50 in step (1) is ≤30 μm; the feeding rate of the prepared raw material in step (2) is 0.1 MC, in g / min, and M is the cross-sectional area of the high temperature chamber, in cm 2 , C is the transmission rate in the high temperature chamber, unit is cm / min.