Gamma-Al2O3 modified red mud catalyst and application thereof
By pickling the red mud and mixing it with γ-Al2O3, a γ-Al2O3 modified red mud catalyst is formed, which solves the problems of Na2O sintering and alumina α phase in red mud, and improves the catalytic decomposition performance and stability of CF4 It realizes efficient utilization of red mud and environmentally friendly CF4 treatment.
Patent Information
- Application Number
- CN202411191248.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
When using red mud as a catalyst in the prior art, the sintering of Na2O leads to pore blockage. After acid treatment, the alumina becomes an α phase, which cannot effectively decompose CF4 gas, and the decomposition effect is not ideal.
By pickling the red mud, its specific surface area and pore structure are improved, and mixed with γ-Al2O3 to calcinate it, a γ-Al2O3 modified red mud catalyst is formed to support the dispersion of γ-Al2O3 and the adsorption and catalytic decomposition of CF4.
It improves the utilization rate of red mud, reduces process costs, enhances the catalytic decomposition performance and stability of CF4, and achieves effective CF4 gas decomposition.
Smart Images

Figure CN119075962A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste resource utilization and industrial flue gas purification, and specifically relates to a γ-Al2O3 modified red mud catalyst and application thereof. Background Art
[0002] Global warming has become one of the most pressing issues of the 21st century. Perfluorocarbons (PFCs) have attracted widespread attention due to their extremely strong greenhouse effect. Their greenhouse effect potential is 6,500 times that of CO2, and their retention time in the atmosphere is as long as 2,600-80,000 years. They are greenhouse gases that are subject to key regulation by international conventions such as the Kyoto Protocol and the Paris Agreement. PFCs mainly include gases such as CF4, C2F6, and C3F8, among which CF4 is the gas that PFCs focus on controlling and is the PFC gas with the highest content. CF4 is a permanent and effective greenhouse gas due to its strong infrared radiation adsorption capacity. At the same time, the highly symmetrical and stable CF bond structure makes the activation of CF4 a huge challenge. However, the global changes caused by CF4 emissions are irreversible on a human time scale, so there is an urgent need for an economical and effective method to deal with it.
[0003] At present, the control of CF4 in the electrolytic aluminum industry is mainly divided into two categories: source reduction and end-of-pipe treatment. The end-of-pipe treatment methods include direct combustion, plasma treatment, adsorption, pyrolysis and catalytic decomposition. Compared with other treatment methods, catalytic decomposition is widely used because of its advantages of low energy consumption, no toxic by-products and simple treatment process.
[0004] Red mud (RM) is a strongly alkaline solid waste generated during the production of alumina. Since RM contains a large amount of metal oxides such as aluminum oxide and iron oxide, it is widely used as a catalyst carrier and catalyst. However, alkaline earth metals such as Na2O in RM will sinter and block the pores of the catalyst, which is not conducive to the CF4 reaction. At the same time, although removing alkaline substances through acid treatment is the key to activating RM for CF4 decomposition, the decomposition effect of RM is not ideal. After acid washing, the aluminum oxide in RM is α phase and has no decomposition effect on CF4. The present invention proposes a method for preparing a catalyst for decomposing CF4 gas by using γ-Al2O3 modified acid-washed red mud. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a γ-Al2O3 modified red mud catalyst and its application.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a γ-Al2O3 modified red mud catalyst, the red mud is acid washed, and the mass ratio of the acid washed red mud to γ-Al2O3 is (1-4):1;
[0007] The preparation method of the γ-Al2O3 modified red mud catalyst comprises the following steps:
[0008] (1) drying and grinding red mud into red mud powder;
[0009] (2) mixing the red mud powder with a hydrochloric acid solution for pickling; then filtering, washing, and drying the pickled red mud to obtain pickled red mud;
[0010] (3) The acid-washed red mud is mixed with γ-Al2O3 and then calcined to obtain a γ-Al2O3 modified red mud catalyst.
[0011] As a preferred embodiment of the present invention, the solid-to-liquid ratio of the red mud powder to the hydrochloric acid solution is 1 g: (6-9) mL.
[0012] As a preferred embodiment of the present invention, the pickling temperature is 80° C. and the time is 240 min.
[0013] As a preferred embodiment of the present invention, the calcination is carried out in an air atmosphere, with the temperature being increased to 650-800° C. at a heating rate of 2° C. / min and kept at this temperature for 5 hours.
[0014] The present invention also claims to protect the use of the γ-Al2O3 modified red mud catalyst in catalytic decomposition of CF4.
[0015] Compared with the prior art, the invention has the following beneficial effects: the invention increases the specific surface area and pore structure of red mud by acid-washing the red mud. Then, the red mud is mixed with γ-Al2O3 and calcined. The acid-washed red mud is used as a carrier to support the γ-Al2O3 and disperse it, which promotes the adsorption of CF4 by Lewis acid sites and the breaking of CF bonds, and improves the stability of the material's catalytic decomposition performance of CF4. The invention uses the method of "treating waste with waste", which not only improves the utilization rate of red mud, but also reduces process costs and reduces pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the preparation process of γ-Al2O3 modified red mud catalyst and its catalytic CF4 flow chart.
[0017] Figure 2 This is the XRD pattern of the catalytic material prepared in Example 1 before and after the CF4 decomposition reaction.
[0018] Figure 3 The SEM image, element content and distribution diagram of the catalytic material prepared in Example 1 after CF4 decomposition reaction.
[0019] Figure 4 This is a stability test of the catalytic material prepared in Example 1. DETAILED DESCRIPTION
[0020] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0021] Example 1
[0022] like Figure 1 , a method for preparing a γ-Al2O3 modified red mud catalyst comprises the following steps:
[0023] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature blast drying oven at 100°C for 24 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0024] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:9, and the beaker was placed in a constant temperature water bath and stirred for 240 min at 80°C. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0025] (3) The acid-washed red mud and γ-Al2O3 were mixed in a mass ratio of 2:1, then placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min under an air atmosphere, and kept warm for 5 h for calcination to obtain a γ-Al2O3 modified red mud catalyst.
[0026] Depend on Figure 2 It can be seen that the catalytic material prepared in Example 1 before the CF4 decomposition reaction contains abundant Al2O3, CaO, and SiO2, and has more acidic sites, which can promote the decomposition of CF4 gas. After the reaction, the CF bond of the catalytic material is broken and forms fluoride with part of the oxide, which remains on the catalyst surface, and the combination with CaF2 is more.
[0027] Depend on Figure 3 It can be seen that after the CF4 decomposition reaction, evenly dispersed F appears on the surface of the catalytic material prepared in Example 1, which proves that the catalytic material prepared by this method has a good decomposition ability for CF4 gas. Figure 2 From the XRD pattern, it can be found that the increase in F content is due to the fluoride formed by the reaction between the CF bond and the oxide after breaking.
[0028] according to Figure 4 It can be seen that the material prepared in Example 1 of the present invention has a good decomposition ability for CF4 gas within 12 hours, indicating that the γ-Al2O3 modified red mud catalyst of the present invention has structural stability and performance stability, and the combination of acid-washed red mud and γ-Al2O3 can improve the stability of the material.
[0029] Example 2
[0030] A method for preparing a γ-Al2O3 modified red mud catalyst comprises the following steps:
[0031] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature forced air drying oven at 100°C for 32 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0032] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:8, and the beaker was placed in a constant temperature water bath and stirred for 240 min at 80°C. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0033] (3) The acid-washed red mud and γ-Al2O3 were mixed in a mass ratio of 1:1, then placed in a muffle furnace, heated to 700°C at a heating rate of 2°C / min under an air atmosphere, and kept warm for 5 h for calcination to obtain a γ-Al2O3 modified red mud catalyst.
[0034] Example 3
[0035] A method for preparing a γ-Al2O3 modified red mud catalyst comprises the following steps:
[0036] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature forced air drying oven at 100°C for 32 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0037] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:7, and the beaker was placed in a constant temperature water bath and stirred at 80°C for 240 min. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0038] (3) The acid-washed red mud and γ-Al2O3 were mixed in a mass ratio of 3:1, then placed in a muffle furnace, heated to 750°C at a heating rate of 2°C / min in an air atmosphere, and kept warm for 5 h for calcination to obtain a γ-Al2O3 modified red mud catalyst.
[0039] Example 4
[0040] A method for preparing a γ-Al2O3 modified red mud catalyst comprises the following steps:
[0041] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature blast drying oven at 100°C for 48 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0042] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:6, and the beaker was placed in a constant temperature water bath and stirred for 240 min at 80°C. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0043] (3) The acid-washed red mud and γ-Al2O3 were mixed in a mass ratio of 4:1, then placed in a muffle furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, and kept warm for 5 h for calcination to obtain a γ-Al2O3 modified red mud catalyst.
[0044] Comparative Example 1
[0045] The only difference between the preparation method of the red mud catalyst described in this comparative example and that in Example 1 is that the acid-washed red mud is not mixed with γ-Al2O3, but directly calcined to prepare the catalyst, comprising the following steps:
[0046] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature blast drying oven at 100°C for 24 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0047] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:9, and the beaker was placed in a constant temperature water bath and stirred for 240 min at 80°C. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0048] (3) The acid-washed red mud was placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min under an air atmosphere, and kept at this temperature for 5 hours for calcination to obtain a modified red mud catalyst.
[0049] Comparative Example 2
[0050] The preparation method of the γ-Al2O3 modified red mud catalyst described in this comparative example is different from that in Example 1 in that the red mud powder is not acid-washed, and the red mud and γ-Al2O3 are directly mixed and roasted, comprising the following steps:
[0051] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature blast drying oven at 100°C for 24 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0052] (2) Red mud powder and γ-Al2O3 were mixed in a mass ratio of 2:1, then placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min under an air atmosphere, and kept warm for 5 h for calcination to obtain a γ-Al2O3 modified red mud catalyst.
[0053] Comparative Example 3
[0054] The preparation method of the γ-Al2O3 catalyst in this comparative example is different from that in Example 1 in that the γ-Al2O3 is not mixed with red mud powder and is directly calcined as a catalyst, and comprises the following steps:
[0055] (1) γ-Al2O3 was placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min in an air atmosphere, and kept at this temperature for 5 h for calcination to obtain a γ-Al2O3 catalyst.
[0056] Comparative Example 4
[0057] A method for preparing a γ-Al2O3 modified red mud catalyst comprises the following steps:
[0058] (1) The Bayer red mud produced by an aluminum company in Wenshan Prefecture, Yunnan Province was dried in an electric constant temperature blast drying oven at 100°C for 24 hours, ground with an agate mortar and sieved through a 100-mesh sieve to obtain red mud powder for later use.
[0059] (2) Red mud powder and 8 mol / L hydrochloric acid were added to a beaker in a solid-liquid ratio of 1:9, and the beaker was placed in a constant temperature water bath and stirred for 240 min at 80°C. The acid-washed red mud was then cooled to room temperature, filtered, and washed with deionized water of 20% of the mass of the red mud powder, and dried in an electric constant temperature blast drying oven at 100°C for 24 h to obtain the acid-washed red mud for use.
[0060] (3) The acid-washed red mud is placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min in an air atmosphere, and kept at this temperature for 5 hours to obtain calcined red mud.
[0061] (4) The γ-Al2O3 was placed in a muffle furnace, heated to 650°C at a heating rate of 2°C / min in an air atmosphere, and kept at this temperature for 5 h to obtain calcined γ-Al2O3.
[0062] (5) The calcined red mud and the calcined γ-Al2O3 were mixed in a mass ratio of 2:1 to obtain a γ-Al2O3 modified red mud catalyst.
[0063] Comparative Example 5
[0064] The only difference between the preparation method of the θ-Al2O3 modified red mud catalyst described in this comparative example and that in Example 1 is that the γ-Al2O3 in step (3) is replaced by an equal mass of θ-Al2O3.
[0065] Comparative Example 6
[0066] The only difference between the preparation method of the γ-Al2O3 modified red mud catalyst described in this comparative example and that in Example 1 is that the red mud in step (3) is replaced by an equal mass of CaO.
[0067] Effect example
[0068] Test samples: catalysts prepared in Examples 1-4 and catalysts prepared in Comparative Examples 1-6.
[0069] Test method: 1.0g of catalyst was placed in a fixed bed reactor, and the reaction temperature gradient was 400-650°C. After the temperature of the fixed bed reactor was raised from 10°C to 400°C, 0.4% CF4 gas was introduced into the reactor through a mixing tank at a gas flow rate of 50mL / min for catalytic decomposition experiments. The outlet gas was detected by gas chromatography. The results of CF4 decomposition efficiency are shown in Table 2.
[0070] Table 2
[0071]
[0072] Compared with Example 1, in Comparative Example 4, the performance of CF4 decomposition was deteriorated after the acid-washed red mud and γ-Al2O3 were first calcined separately and then the catalytic material was prepared by physical mixing. The contact and interaction between the active components were weak when the acid-washed red mud and γ-Al2O3 were calcined separately and then physically mixed, and the active components were unevenly distributed, and even pore blockage or disconnected pore structure occurred, which affected the material performance.
[0073] Compared with Example 1, after using θ-Al2O3 as the active component in Comparative Example 5, the decomposition performance of CF4 is reduced. Compared with θ-Al2O3 combined with red mud catalyst, γ-Al2O3 combined with red mud catalyst has a stronger ability to activate CF4, mainly because γ-Al2O3 combined with red mud catalyst has more AlⅢ The activation of CF by (the strongest Lewis acid site) is beneficial to the diffusion and adsorption of CF4.
[0074] Compared with Example 1, Comparative Example 6 replaces red mud with an equal mass of CaO, and the performance is similar to that of γ-Al2O3 alone, but it is quite different from the performance of the material prepared by mixing acid-washed red mud and γ-Al2O3. CF4 usually requires more Lewis acid sites to break the CF bonds during the decomposition process, and CaO, as an alkaline substance, lacks active sites, and its low specific surface area and pore structure lead to a decrease in the contact sites between CF4 and the material surface. The main components of red mud are aluminum oxide, calcium oxide, and iron oxide. After acid washing, not only the alkaline components are removed, but also the specific surface area is increased and the pore structure is adjusted, which helps to evenly disperse the active components on the carrier surface.
[0075] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A γ-Al2O3 modified red mud catalyst, characterized in that: After the red mud is pickled, the mass ratio of the pickled red mud to γ-Al2O3 is (1-4):1; The preparation method of the γ-Al2O3 modified red mud catalyst comprises the following steps: (1) drying and grinding red mud into red mud powder; (2) mixing the red mud powder with a hydrochloric acid solution for pickling; then filtering, washing, and drying the pickled red mud to obtain pickled red mud; (3) The acid-washed red mud is mixed with γ-Al2O3 and then calcined to obtain a γ-Al2O3 modified red mud catalyst.
2. The γ-Al2O3 modified red mud catalyst according to claim 1, characterized in that: The solid-to-liquid ratio of the red mud powder to the hydrochloric acid solution is 1 g: (6-9) mL.
3. The γ-Al2O3 modified red mud catalyst according to claim 1, characterized in that: The pickling temperature is 80° C. and the time is 240 min.
4. The γ-Al2O3 modified red mud catalyst according to claim 1, characterized in that: The calcination is carried out in an air atmosphere, with the temperature being increased to 650-800° C. at a heating rate of 2° C. / min, and the temperature being kept for 5 hours.
5. Use of the γ-Al2O3 modified red mud catalyst as described in any one of claims 1 to 4 in catalytic decomposition of CF4.