Nano-diamond catalytic material as well as preparation method and application thereof

The nanodiamond catalytic material prepared by calcination at 700-1500°C combined with persulfate is solved, and the problem of endocrine interference removal in wastewater is achieved, achieving efficient wastewater treatment effect.

CN119075965APending Publication Date: 2024-12-06CHINA CONSTR THIRD ENG BUREAU GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092418.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

There is no application of nanodiamond in the prior art in wastewater treatment, especially in removing endocrine disturbances in water bodies.

Method used

By calcining nanodiamond under a protective atmosphere of 700-1500°C, a nanodiamond catalytic material with sp2 hybrid carbon atoms and π electrons was prepared, and combined with persulfate to remove endocrine disturbances in water. Such as bisphenol A.

Benefits of technology

A simple preparation method is realized, the catalytic activity of nanodiamond catalytic materials is improved, and the endocrine interference in water can be effectively removed, which significantly improves the effect of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075965A_ABST
    Figure CN119075965A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a nano-diamond catalytic material, and belongs to the technical field of environmental pollution treatment. The nano-diamond catalytic material has sp2 hybrid carbon atoms and pi electrons; the nano-diamond catalytic material is used for removing endocrine disrupters in a water body. The nano-diamond catalytic material provided by the invention can activate persulfate to remove endocrine disrupters in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental pollution control, and in particular to a nano-diamond catalytic material and a preparation method and application thereof. Background Art

[0002] Nanodiamond, the only nanomaterial composed of sp3 hybridized carbon atoms among carbon-based nanomaterials, was developed more than 30 years ago, but its application was limited to abrasives such as polycrystalline and polishing agents. With the deepening of people's understanding of the properties of nanodiamonds, nanodiamonds have begun to be used in lubricating oils, metal coatings, magnetic recording systems, medicine and other fields, and the application fields are still expanding. In the existing technology, there is no application of nanodiamonds in wastewater treatment. Summary of the invention

[0003] In view of the deficiencies of the above prior art, the first aspect of the present invention provides a method for preparing a nano-diamond catalytic material. The second aspect of the present invention provides a nano-diamond catalytic material. The third aspect of the present invention provides an application of a nano-diamond catalytic material. The preparation method of the nano-diamond catalytic material of the present invention is simple and easy to operate. The obtained nano-diamond catalytic material has sp2 hybridized carbon atoms and π electrons, and can catalyze the oxidation of persulfate to remove endocrine disruptors in water. It is specifically achieved through the following technologies.

[0004] A first aspect of the present invention provides a nano-diamond catalytic material, comprising sp2 hybridized carbon atoms and π electrons; the nano-diamond catalytic material is used to remove endocrine disruptors in water.

[0005] A second aspect of the present invention provides a method for preparing a nano-diamond catalytic material, comprising the following steps:

[0006] The nano-diamond is placed in a sealed container, and calcined at 700-1500° C. in a protective gas atmosphere for a calcination time of not less than 4 hours to obtain a nano-diamond catalytic material;

[0007] The nano diamond catalytic material is used for removing endocrine disruptors in water.

[0008] Furthermore, the container is any one of an alumina boat, a graphite boat, and a corundum boat.

[0009] Furthermore, the sealing is performed by using aluminum foil to seal the alumina boat.

[0010] Furthermore, the calcination conditions are: temperature of 700-1500° C. and time of not less than 4 hours.

[0011] Furthermore, the calcination condition is: the temperature is 1100-1500°C.

[0012] Furthermore, when the calcination temperature is 700-1000°C, the heating / cooling rate is 10°C / min.

[0013] Furthermore, when the calcination temperature is higher than 1000° C., the heating / cooling rate is 5° C. / min.

[0014] A third aspect of the present invention provides an application of a nano-diamond catalytic material for removing endocrine disruptors in water.

[0015] Furthermore, nano-diamond catalytic materials and persulfate are added to the water body to remove endocrine disruptors in the water body.

[0016] Furthermore, the endocrine disruptor includes at least one of bisphenol A, bisphenol AF, and bisphenol S.

[0017] Compared with the prior art, the present invention is beneficial in that:

[0018] The preparation method of the nano-diamond catalytic material of the present invention is simple and easy to operate. The obtained nano-diamond catalytic material has sp2 hybridized carbon atoms and π electrons and can catalyze the oxidation of persulfate to remove endocrine disruptors in water, such as bisphenol A. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The SEM images of each group of nanodiamond catalytic materials;

[0020] Figure 2 The EDS images of each group of nanodiamond catalytic materials;

[0021] Figure 3 A comparison of the oxygen content of different types of NDs in the EDS characterization of each group of nanodiamond catalytic materials;

[0022] Figure 4 FTIR images of each group of nanodiamond catalytic materials;

[0023] Figure 5 XRD patterns of each group of nanodiamond catalytic materials;

[0024] Figure 6 XRD comparison diagram of each group of nanodiamond catalytic materials;

[0025] Figure 7 The Raman images of each group of nanodiamond catalytic materials;

[0026] Figure 8 The EPR images of each group of nanodiamond catalytic materials;

[0027] Fig. 9The conductivity diagram of each group of nanodiamond catalytic materials;

[0028] Fig.10 This is a comparison chart of the effects of each group of nano-diamond catalytic materials on activating PS to remove BPA;

[0029] Fig.11 This is a comparison chart of the degradation efficiency of each group of nanodiamond catalytic materials under different initial PS concentrations;

[0030] Fig.12 This is a comparison chart of the effects of different nano-diamond catalytic material dosages on the removal efficiency of BPA;

[0031] Fig.13 This is a comparison chart of the degradation efficiency of each group of nanodiamond catalytic materials under different initial BPA concentrations;

[0032] Fig.14 This is a comparison chart of the degradation efficiency of each group of nanodiamond catalytic materials under different initial pH values. DETAILED DESCRIPTION

[0033] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0034] The present invention provides an exemplary method for preparing a nano-diamond catalytic material, comprising the following steps:

[0035] The nano-diamond is placed in a sealed container, and calcined at 700-1500° C. in a protective gas atmosphere for a calcination time of not less than 4 hours to obtain a nano-diamond catalytic material;

[0036] The nano diamond catalytic material is used for removing endocrine disruptors in water.

[0037] In some examples of the present invention, the container may be any one of an alumina boat, a graphite boat, and a corundum boat.

[0038] In some examples of the present invention, the sealing may be performed by sealing an alumina boat using aluminum foil.

[0039] In some examples of the present invention, the protective gas may include at least one of argon, helium, and nitrogen.

[0040] In some examples of the present invention, the calcination conditions may be: a temperature of 700-1500° C. and a time of not less than 4 hours.

[0041] In some examples of the present invention, the calcination conditions may be: a temperature of 1100-1500° C. and a time of not less than 4 hours.

[0042] In some examples of the present invention, when the calcination temperature is 700-1000° C., the heating / cooling rate may be 10° C. / min.

[0043] In some examples of the present invention, when the calcination temperature is higher than 1000° C., the heating / cooling rate may be 5° C. / min.

[0044] The present invention also exemplarily provides an application of a nano-diamond catalytic material for removing endocrine disruptors in water.

[0045] In some examples of the present invention, nanodiamond catalytic materials and persulfate can be added to water to remove endocrine disruptors in the water.

[0046] In some examples of the present invention, the endocrine disruptor may include at least one of bisphenol A, bisphenol AF, and bisphenol S.

[0047] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] The present invention exemplarily provides a method for preparing a nano-diamond catalytic material, comprising the following steps:

[0049] S1. Commercially purchased nanodiamonds were placed in an alumina boat and sealed with aluminum foil;

[0050] S2. Place the sealed alumina boat in step S1 into a high-temperature tube furnace, and calcine for 4 hours under the protection of an argon atmosphere with an argon flow rate of 0.1 L / min to obtain a nano-diamond catalytic material.

[0051] In a specific embodiment of the present invention, the sealed alumina boat in step S1 is calcined at 300°C, 500°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C and 1500°C, respectively. The nano-diamond catalytic materials obtained after calcination are marked as ND-300, ND-500, ND-700, ND-800, ND-900, ND-1000, ND-1100, ND-1200, ND-1300, ND-1400 and ND-1500, for a total of 11 groups. The calcination parameters of each group are shown in Table 1 below. The heating rates of each group: 0→1000°C, 10°C / min; 1000→1500°C, 5°C / min. Cooling rate of each group: 1000→0℃, 10℃ / min; 1500→1000℃, 5℃ / min.

[0052] Table 1 Calcination parameters of each group

[0053] 1. SEM test

[0054] The nanodiamond catalytic materials obtained from the above 11 groups and the uncalcined nanodiamond (marked as ND) were subjected to electron microscope scanning to obtain the SEM images of each group as shown in the following figure: Figure 1 shown.

[0055] Depend on Figure 1 (a) It can be seen that the unmodified nanodiamond (ND) is in a typical granular shape (spherical or ellipsoidal) and is irregularly aggregated. However, after ND is treated at high temperature, its morphological characteristics are found to have slight changes: Figure 1 (b)- Figure 1 (l) It can be seen that with the increase of calcination temperature (300-1500℃), the nanodiamond microscopic particles gradually change from spherical or ellipsoidal to lamellar, indicating that during the high-temperature treatment process, ND gradually changes from cubic diamond phase to graphite phase with the increase of temperature. The change of its apparent color (from light gray to dark black) can also illustrate this point.

[0056] 2. EDS test

[0057] The 11 groups of nanodiamond catalytic materials and uncalcined nanodiamonds were tested by Energy Dispersive Spectrometer (EDS), and the EDS graphs of each group were obtained as shown in Figure 2-3 shown.

[0058] Figure 2 The EDS images of various groups of nanodiamond catalytic materials are shown in Figure 2. Theoretically, nanodiamond is an allotrope of carbon and should be composed of pure carbon. However, Figure 2 The results show that the main components of ND are C and O elements, of which C is the main element and O only accounts for a small part. This is mainly because some oxygen-containing functional groups (such as carbonyl, hydroxyl, carboxyl, ester, etc.) will inevitably be generated and remain on the surface of nanodiamonds during the preparation and storage of nanodiamonds. With the increase of treatment temperature, the proportion of oxygen contained in ND decreases continuously. This is mainly because the heat energy at high temperature causes the carbon-oxygen bond to break, resulting in the loss of oxygen elements; and the bond energy of carbon-oxygen bonds in different oxygen-containing functional groups is different, resulting in inconsistent critical temperatures for bond breaking.

[0059] Figure 3 The figure shows the oxygen content comparison of different types of ND in the EDS characterization of each group of nanodiamond catalytic materials. Figure 3As shown, it indicates that with the increase of temperature, different types of oxygen-containing functional groups on the ND surface are gradually removed, resulting in a continuous decrease in oxygen content.

[0060] 3. FTIR test

[0061] The nanodiamond catalytic materials and uncalcined nanodiamonds obtained in the above 11 groups were subjected to Fourier transform infrared spectroscopy (FTIR) testing, and the FTIR graphs of each group were obtained as shown in the following figure: Figure 4 shown.

[0062] In the present invention, FTIR is used to characterize and analyze different types of nanodiamonds (ND to ND-1500). Figure 4 It can be seen that the uncalcined ND is in the range of 800-3600cm -1 There are four obvious reaction peaks in the wavelength range of 1083cm -1 、1680cm -1 、2933cm -1 , and 3432cm -1 , representing carbon-oxygen single bond (CO), carbon-oxygen double bond (C=O), carbon-hydrogen bond (CH) and hydrogen-oxygen bond (OH). With the increase of calcination temperature, the content of various functional groups on the ND surface gradually decreases. When the calcination temperature reaches 1300°C, almost no functional groups are detected on the surface of nanodiamonds, which is consistent with the conclusion of EDS. It is worth mentioning that in the EDS test results, ND-1300, ND-1400 and ND-1500 still contain some oxygen elements, which is mainly due to the influence of oxygen in the air. This is caused by the defects of the characterization instrument itself and is generally unavoidable.

[0063] 4. XRD test

[0064] The nanodiamond catalytic materials obtained in the above 11 groups and the uncalcined nanodiamonds were subjected to X-ray diffraction analysis and testing, and the XRD patterns of each group were obtained as follows: Figure 5-6 shown.

[0065] In order to determine the phase and composition of nanodiamonds during high-temperature thermal phase transition, the present invention uses XRD to characterize the structure of each group of nanodiamonds to obtain Figure 5 and Figure 6 .from Figure 5 Typical diamond diffraction peaks can be observed in (a), among which 2θ≈43.7° is the characteristic diffraction peak of the diamond (111) plane; and 2θ≈75.8° is the characteristic diffraction peak of the diamond (220) plane. Apart from these, there are no other obvious diffraction peaks, and the baseline is stable and smooth, indicating that the raw material nanodiamond has a high purity, is free of other impurities, and is almost entirely composed of sp3 hybridized carbon atoms.

[0066] However, after a series of high-temperature treatments, the crystal structure of ND has changed to a certain extent. Figure 5 (b)- Figure 5 (l) and Figure 6 It can be seen that with the increase of calcination temperature, the diffraction peak intensity of diamond (111) plane and diamond (220) plane gradually decreases, indicating that the proportion of carbon atoms in the sp3 diamond phase gradually decreases, and when the temperature reaches 1500℃, the two diffraction peaks almost disappear, indicating that after the nanodiamond is treated under this temperature condition, the hybridization mode of its internal carbon atoms is almost completely converted from sp3 hybridization to other types of carbon atoms. When the treatment temperature is greater than or equal to 1100℃, a new diffraction peak appears at 2θ≈25.3°, which is the characteristic diffraction peak of the (002) plane of graphite phase carbon (composed of sp2 hybridized carbon atoms), and its peak intensity increases with the increase of calcination temperature, indicating that the raw material nanodiamond mainly composed of sp3 hybridized carbon atoms is calcined at 300-1500℃, and as the treatment temperature increases, its internal carbon atoms gradually transform from sp3 hybridization to sp2 hybridization.

[0067] 5. Raman test

[0068] The nanodiamond catalytic materials and uncalcined nanodiamonds obtained from the above 11 groups were subjected to laser Raman spectroscopy test, and the Raman spectra of each group were obtained as shown in Figure 7 shown.

[0069] In the laser Raman analysis of carbon materials of the present invention, the excitation wavelength is 532nm, which belongs to the visible light range, and the spectrum mainly depends on the composition of sp2 hybridized carbon atoms. This is mainly because visible light laser can only resonate with the π electrons of the C=C double bond in the carbon material. Figure 7 As shown in (a), nanodiamond (ND) and nanodiamonds calcined at temperatures below 700°C (ND300, ND500 and ND-700) have no obvious Raman peaks, and the spectra of each group do not change much, indicating that when the temperature is below 700°C, the calcination treatment has little effect on the carbon atom composition structure inside ND, and the main elementary structure is still a regular tetragonal cube composed of sp3 hybridized carbon atoms.

[0070] like Figure 7 As shown in (b), when the treatment temperature is higher than 700℃, two typical D and G peaks of sp2 hybridized carbon materials appear in the Raman spectrum. In addition, when the treatment temperature is higher than 1300℃, a peak at 2685cm -1 A 2D peak appears at

[0071] Among them, the D peak is usually considered to be the disordered vibration peak of sp2 carbon nanomaterials, which appears at 1325 cm -1The inelastic valley scattering of iTO phonons near the K point and the valley scattering of a defect are involved, that is, the defect will activate the breathing vibration mode of the six-membered ring and lead to the corresponding Raman active peak. It is caused by the lattice vibration leaving the center of the Brillouin zone and is used to characterize the structural defects or edges in the graphene sample.

[0072] The G peak is usually considered to be the characteristic peak of sp2 hybridized carbon atoms, which appears at 1585 cm -1 Nearby, it involves the intravalley scattering process of two doubly degenerate iTO and iLO phonons near the Γ point. This peak is generally generated by the in-plane vibration of sp2 carbon atoms, and the corresponding vibration mode has E2g symmetry.

[0073] The 2D peak is a two-phonon resonance second-order Raman peak, which is generated by two valley inelastic scatterings of an iTO phonon near the K point. As a two-phonon resonance Raman peak, it is often believed that this peak has nothing to do with defects, but it has a great correlation with the layer structure and stacking mode, and can also be used as a characteristic peak of sp2 hybridized carbon nanomaterials.

[0074] In addition, with the increase of treatment temperature (800-1500℃), the peak intensities of D peak, G peak and 2D peak become higher and higher, and the peak shapes become better and better, indicating that the nanodiamond composed of sp3 hybridized carbon atoms begins to undergo phase change from 800℃ under high-temperature calcination treatment, and the carbon atoms gradually transform from sp3 hybridization to sp2 hybridization, and with the increase of treatment temperature, the proportion of sp2 hybridized carbon atoms continues to increase.

[0075] By locally enlarging the Raman spectrum, such as Figure 7 As shown in (c), it is not difficult to find that with the continuous increase of the treatment temperature, the positions of the D peak and the G peak shift to a certain extent, and their peak shapes become narrower and narrower, indicating that the disorder of the catalyst gradually decreases and gradually transforms into a high-purity sp2 hybridized carbon-based material.

[0076] 6. EPR test

[0077] The nanodiamond catalytic materials obtained in the above 11 groups and the uncalcined nanodiamonds were subjected to electron paramagnetic resonance (EPR) tests, and the EPR patterns of each group were obtained as shown in FIG. Figure 8 shown.

[0078] EPR can directly characterize and analyze nanodiamond catalytic materials to provide relevant information about dangling bonds and unpaired electrons in nanodiamond catalytic materials. Figure 8As shown in (a), when the treatment temperature is lower than 1100℃, the EPR signal intensity decreases slowly; when the treatment temperature is higher than 1100℃, the signal intensity decreases significantly, especially when the temperature reaches 1500℃, the EPR signal is almost undetectable. This indicates that the recombination of dangling bonds on the ND surface leads to a reduction in unpaired electrons; however, after high-temperature calcination of ND, the reorganized dangling bonds inside it will cause the generation of π electrons. Figure 8 As shown in (d), when the temperature is higher than 1100℃, its g value suddenly drops steeply, which indicates that the π electrons inside the nanodiamond catalytic material of the ND-1100 group begin to transform from localized electrons to delocalized electrons. When the calcination temperature is 1500℃, the degree of delocalization of π electrons inside the nanodiamond catalytic material reaches its peak.

[0079] 7. Conductivity test

[0080] The conductivity of the nanodiamond catalytic materials and uncalcined nanodiamond obtained in the above 11 groups was measured by the four-probe method, and the conductivity values ​​of ND, ND-300, ND-500, ND-700, ND-800, ND-900, ND-1000, ND-1100, ND-1200, ND-1300, ND-1400 and ND-1500 were 0.021S / cm, 0.023S / cm, 0.027S / cm, 0.039S / cm, 0.088S / cm, 0.153S / cm, 0.252S / cm, 0.689S / cm, 1.307S / cm, 1.548S / cm, 2.539S / cm and 2.823S / cm, respectively. The conductivity results of each group are as follows: Fig. 9 shown.

[0081] like Fig. 9 As shown in the figure, in general, high temperature treatment can significantly improve the conductivity of ND, and it increases with the increase of treatment temperature. In fact, when the treatment temperature is lower than 800℃, its conductivity hardly changes, which is mainly due to the desorption of water molecules on the surface of ND and the removal of oxygen-containing functional groups in this process; when the temperature is higher than 800℃, the conductivity begins to increase significantly, which is mainly due to the gradual transformation of carbon atoms inside nanodiamonds from sp3 hybridization to sp2 electrons, resulting in an increase in π electrons and conducive to the improvement of electrical properties; and when the temperature is higher than 1100℃, the rate of improvement of its conductivity is further improved, which is mainly due to the delocalization of π electrons inside the catalyst, which enables it to move freely in the large π bonds formed in the entire catalyst system, and its electrical properties are further improved.

[0082] Application example: Catalytic degradation test

[0083] Prepare 12 groups of identical solution systems: prepare 100 mL of 0.1 mM BPA solution, place it in a magnetic stirrer, and add 0.2 mM sodium persulfate (PS) solution. Then add 0.005 g of nano-diamond catalytic material respectively, and only add one nano-diamond catalytic material to each group. In each group, the concentration of nano-diamond catalytic material is 0.05 g / L. Start the reaction, and the reaction time is 30 min. The pH value is not adjusted, and the initial pH value is 6.1. After the reaction time, the terminator Na2SO3 is added to each group. After the reaction is completed, each group is sampled and placed in a centrifuge and spun at high speed at 13000 rpm for 3 minutes. After centrifugation, the sample is used to determine the remaining BPA concentration by high performance liquid chromatography. The experiment was repeated three times and the average value was taken to avoid errors. The results are as follows Fig.10 shown.

[0084] Depend on Fig.10 (a) It can be seen that the higher the temperature of nanodiamond calcination, the higher the oxidation removal efficiency of BPA by the obtained nanodiamond catalytic material. Fig.10 (b) It can be seen that the pseudo-first-order kinetic constants of the nanodiamond catalytic materials of ND, ND-300, ND-500, ND-700, ND-800, ND-900, ND-1000, ND-1100, ND-1200, ND-1300, ND-1400 and ND-1500 for activating PS to remove BPA are 0.0116 min -1 、0.0171min -1 、0.0342min -1 、0.0551min -1 、0.0801min -1 、0.1149min -1 、0.1532min -1 、0.1848min -1 、0.2342min -1 、0.3162min -1 、0.4263min -1 and 0.6481min -1 The results show that as the carbon atoms in the nanodiamond material continue to transform from sp3 hybridization to sp2 hybridization, it is beneficial to its activation of PS to oxidize and degrade organic pollutants in water.

[0085] Based on the above catalytic degradation test, the present invention also conducted the following comparative test:

[0086] Comparative experiment 1: Degradation performance test of nanodiamond catalytic materials at different PS initial concentrations

[0087] On the basis of the above catalytic degradation test, the present invention investigated the degradation efficiency of each group of nano-diamond catalytic materials on BPA under different initial PS concentrations under certain conditions of BPA and nano-diamond catalytic material dosage. (Experimental conditions: [nano-diamond catalytic material] = 0.05g / L, [BPA] = 0.1mM, [PS] = 0.1-0.5mM). After the reaction time, the terminator Na2SO3 was added to each group. After the reaction of each group was completed, each group was sampled and placed in a centrifuge and spun at a high speed of 13000rpm for 3 minutes. After centrifugation, the samples were used to measure the remaining BPA concentration using a high performance liquid chromatograph. The experiment was repeated three times and the average value was taken to avoid errors. The degradation efficiency results of each group are shown as follows. Fig.11 shown.

[0088] Depend on Fig.11 It can be seen that in each group of nanodiamond catalytic material activated PS system, as the amount of PS added increases, the oxidation removal efficiency of BPA also increases. This is mainly because the more PS molecules there are in the system, the higher the probability of collision with the nanodiamond catalytic material, and with the help of the bridge effect of the nanodiamond catalytic material, it can capture the electrons of BPA. Fig.11 (h)- Fig.11 (l) It can also be seen that when the calcination temperature reaches 1100°C, the concentration of BPA decreases faster. This is because after the nanodiamond catalytic material is calcined at a temperature not lower than 1100°C, it can react with more PS molecules, thereby increasing the rate of generating singlet oxygen, leading to accelerated oxidative degradation of BPA.

[0089] Comparative test 2: Test on the effect of different nanodiamond catalytic material dosage on BPA removal efficiency

[0090] Based on the above catalytic degradation test, the present invention investigates the effect of different dosages of nano-diamond catalytic materials on the removal efficiency of BPA. (Experimental conditions: [nano-diamond catalytic material] = 0.02-0.10 g / L, [BPA] = 0.1 mM, [PS] = 0.2 mM). After the reaction time, the terminator Na2SO3 was added to each group. After the reaction of each group was completed, each group was sampled and placed in a centrifuge and spun at 13000 rpm for 3 minutes. After centrifugation, the samples were used to measure the remaining BPA concentration using a high performance liquid chromatograph. The experiment was repeated three times and the average value was taken to avoid errors. The degradation efficiency results of each group are shown in the figure. Fig.12 shown.

[0091] Depend on Fig.12 It can be seen that with the increase in the dosage of nanodiamond catalytic material, its removal performance of BPA is significantly improved within 30 minutes. Fig.12 (a)- Fig.12(d) It can also be seen that although the dosage of nanodiamond catalytic material is greatly increased, ND~ND-700 still cannot activate PS to completely remove BPA within 30 minutes. This is mainly because after the nanodiamond is calcined at a temperature less than or equal to 700°C, there are still a large number of sp3 hybridized carbon atoms in it. Therefore, the electrical conductivity of the nanodiamond catalytic material is low and its own catalytic performance is poor.

[0092] Comparative experiment 3: Degradation performance test of nanodiamond catalytic materials at different initial BPA concentrations

[0093] Considering that the initial concentration of environmental pollutants in the incoming water has an important impact on the practical application of water treatment and wastewater treatment, it directly determines the choice of treatment process in the treatment plant and the choice and dosage of reagents. Therefore, based on the above-mentioned catalytic degradation test, the present invention investigates the degradation efficiency of different initial BPA concentrations under constant dosage conditions of PS and nano-diamond catalytic materials. (Experimental conditions: [nano-diamond catalytic material] = 0.05g / L, [BPA] = 0.05-0.2mM, [PS] = 0.2mM). After the reaction time, the terminator Na2SO3 was added to each group. After the reaction of each group was completed, each group was sampled and placed in a centrifuge and spun at a high speed of 13000rpm for 3min. After centrifugation, the sample was used to determine the residual BPA concentration by high performance liquid chromatography. The experiment was repeated three times and the average value was taken to avoid errors. The degradation efficiency results of each group are shown as follows. Fig.13 shown.

[0094] Depend on Fig.13 It can be seen that as the initial concentration of BPA increases, the degradation rate of BPA by the nanodiamond catalytic materials in each group decreases significantly. This is mainly due to the decrease in the molar ratio of PS to BPA, which leads to a decrease in the collision probability of the unit concentration pollutant and the active substance, thereby inhibiting the oxidative degradation of BPA. Fig.13 (l) It can be seen that when the initial concentration of BPA is 0.2 mM, even the nanodiamond catalytic material that has been calcined at 1500°C cannot completely remove BPA within 30 minutes, and the BPA concentration has no trend of continuing to decrease, which also indicates that the overall reaction coefficient ratio of PS to BPA in this system is greater than 1.

[0095] Comparative test 4: Degradation efficiency test of nanodiamond catalytic material at different initial pH values ​​In sewage treatment, the actual wastewater is generally a mixed liquid with a wide pH range. On the basis of the above-mentioned catalytic degradation test, the present invention investigates the removal efficiency of BPA at different initial pH values ​​under standard conditions ([nanodiamond catalytic material] = 0.05g / L, [BPA] = 0.1mM, [PS] = 0.2mM), and investigates pH values ​​of 3, 5, 7, and 9. After the reaction time, the terminator Na2SO3 was added to each group. After the reaction of each group was completed, each group was sampled and placed in a centrifuge and spun at a high speed of 13000rpm for 3 minutes. After centrifugation, the samples were used to determine the residual BPA concentration using a high performance liquid chromatograph. The experiment was repeated three times and the average value was taken to avoid errors. The degradation efficiency results of each group are shown as follows Fig.14 shown.

[0096] Depend on Fig.14 (a)- Fig.14 (h) It can be seen that when the treatment temperature is lower than 1100℃, the removal efficiency of BPA gradually increases; Fig.14 (i)- Fig.14 (l) It can be seen that when the treatment temperature is higher than 1100℃, the removal rate of BPA increases first and then decreases. The effect of initial pH concentration on BPA removal efficiency is a complex factor, which is mainly related to the pKa value of BPA, pHPZC (pH value of zero charge point) of nanodiamond catalytic material, and the protonation / deprotonation state of active oxygen. However, 1100℃ is the turning point of the influence trend, which further shows the key role of π electron delocalization.

[0097] The above specific embodiments describe the implementation of the present invention in detail, but the present invention is not limited to the specific details in the above embodiments. Within the scope of the claims and technical concept of the present invention, the technical solution of the present invention can be modified and changed in many simple ways, and these simple modifications all belong to the protection scope of the present invention.

Claims

1. A nano-diamond catalytic material, It is characterized in that The nano-diamond catalytic material has sp2 hybridized carbon atoms and π electrons; the nano-diamond catalytic material is used for removing endocrine disruptors in water.

2. The method for preparing the nano-diamond catalytic material according to claim 1, It is characterized in that The following steps are involved: The nano-diamond is placed in a sealed container, and calcined at 700-1500° C. in a protective gas atmosphere for a calcination time of not less than 4 hours to obtain a nano-diamond catalytic material; The nano diamond catalytic material is used for removing endocrine disruptors in water.

3. The preparation method according to claim 2, It is characterized in that The calcination temperature is 1100-1500°C.

4. The preparation method according to claim 2, It is characterized in that When the calcination temperature is 700-1000°C, the heating / cooling rate is 10°C / min.

5. The preparation method according to claim 2, It is characterized in that When the calcination temperature is higher than 1000° C., the heating / cooling rate is 5° C. / min.

6. Use of the nano-diamond catalytic material according to claim 1 to remove endocrine disruptors in water.

7. The use according to claim 6, It is characterized in that The nano-diamond catalytic material and persulfate are added into a water body to remove endocrine disruptors in the water body.

8. The use according to claim 7, It is characterized in that The initial pH value in the water body is 3-9.

9. The use according to claim 7, It is characterized in that The persulfate includes at least one of peroxydisulfate and peroxymonosulfate.