Preparation method of novel efficient antifouling electrode
By mixing metal powder, antifouling agent powder with polymer material powder and preparing through isostatic molding process, the problem of low antifouling ion release efficiency of existing antifouling electrodes is solved, and a variety of high-efficiency and stable antifouling is achieved The agent is released, improving the anti-fouling effect.
Patent Information
- Application Number
- CN202411178370.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The existing antifouling electrodes are made of copper alloy as the main material, and there is a single release of antifouling ions and a slow release efficiency, which affects the antifouling effect.
Using the mixed preparation method of metal powder, antifouling agent powder and polymer material powder, antifouling electrodes with excellent mechanical properties and efficient antifouling ion release are prepared through isostatic molding technology, including copper powder, aluminum powder and antifouling Agents such as cuprous oxide, Econea, etc. are filled into the foam metal to form an efficient antifouling electrode.
The anti-fouling ion release efficiency is significantly improved, and the release efficiency of conventional anti-fouling copper electrodes is increased by more than 50%, meeting the anti-fouling needs of marine facilities and equipment, and the preparation process is scientific and reliable.
Smart Images

Figure BDA0005011377630000051 
Figure BDA0005011377630000052 
Figure BDA0005011377630000061
Abstract
Description
Technical field:
[0001] The present invention belongs to the technical field of marine antifouling, and specifically relates to a method for preparing a novel antifouling electrode with high-efficiency antifouling function, which meets the antifouling needs in the marine field. Background technology:
[0002] Marine biofouling is a common problem in facilities and equipment in the marine environment. Biofouling of underwater facilities may not only cause corrosion of facility materials, but also increase the resistance of ships and block the pipelines of coastal power station cooling systems, thus affecting the normal functions of important facilities and equipment, resulting in significant economic losses and affecting the ecological environment.
[0003] Electrolytic heavy metal antifouling and self-coupling antifouling in the prior art are important antifouling means for underwater marine facilities. The former mainly utilizes the toxic heavy metal ions produced by the electrolytic anode material to inhibit and kill fouling organisms, while the latter is based on the principle of galvanic corrosion, connecting an anode with a more positive potential with a cathode with a more negative potential, and utilizing the potential difference between the two to accelerate the dissolution of toxic heavy metal ions at the anode to achieve the purpose of antifouling.
[0004] At present, the most widely used anode materials are copper and its alloys. Copper anodes can generate toxic copper ions during electrochemical reactions, which kill marine organisms. With the development of marine economy and society, various new underwater marine facilities and equipment are constantly being put into use, which puts forward higher and higher requirements for anti-fouling technology. For example, Chinese patent 202110541987.8 discloses a long-life self-driven anti-fouling device for a ship's seawater box environment without power supply, which consists of an anti-fouling electrode and a mounting base. The anti-fouling electrode is the main functional structure, and the potential difference between dissimilar metals is used to drive the accelerated dissolution of the cathode plate to produce copper ions with an effective anti-fouling concentration; the anti-fouling electrode is composed of a cathode metal plate, an anode metal plate, a clamp, and a fastener. The cathode metal plate and the anode metal plate are fixed by clamps and fasteners at both ends. The number of fasteners is determined by the total number of anode and cathode plates, so that each anode and cathode plate is fixed and not loose; the cathode metal plate is made of an inert metal material, and the anode metal plate is selected from pure copper, red copper, bronze, brass or copper alloys doped with other metal elements. The material of the clamp is consistent with that of the anode metal plate. However, the anti-fouling electrode with copper alloy as the main material in the above patents and prior art has the problem of single anti-fouling ion release and slow release efficiency, which seriously affects the anti-fouling effect. Therefore, in order to solve the above problems, it is necessary to develop and design a method for preparing an antifouling electrode with excellent mechanical properties, which can stably, reliably and efficiently release a variety of antifouling ions and has conductive properties. Summary of the invention:
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and to develop a new method for preparing an efficient antifouling electrode, so as to prepare an antifouling electrode with excellent mechanical properties and the ability to stably, reliably and efficiently release a variety of antifouling ions and conductive properties.
[0006] In order to achieve the above-mentioned purpose, the specific process of the antifouling electrode preparation method of the present invention is as follows:
[0007] (1) mixing metal powder and antifouling agent powder uniformly to obtain antifouling powder;
[0008] The metal powder is one or more metal powders that can be corroded and dissolved in seawater, including copper powder, aluminum powder, iron powder, etc.;
[0009] The antifouling agent powder is one or more of organic and inorganic antifouling agents, including cuprous oxide, cuprous thiocyanate, zinc oxide, copper sulfate, copper naphthenate, acid copper, organic tin, DDT (bis(p-chlorophenyl)trichloroethane), Econea (bromopyrrole nitrile), zinc pyrithione, pyridine triphenyl borane, etc.;
[0010] The weight ratio of antifouling agent powder to metal powder is 0-2:1;
[0011] (2) mixing the antifouling powder and the polymer material powder uniformly to obtain a plastic antifouling powder;
[0012] The polymer material powder is one or more materials that can melt at a certain temperature, including polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic plastics, other polyolefins and copolymers thereof, polysulfone, polyphenylene ether, chlorinated polyether, etc.
[0013] The weight ratio of polymer material powder to antifouling powder is 0-0.2:1;
[0014] (3) filling the plastic antifouling powder into the foam metal to obtain an antifouling electrode precursor;
[0015] Wherein, the foam metal is one or more of foam copper, foam nickel, and foam aluminum;
[0016] (4) pressing the antifouling electrode precursor into an antifouling electrode by isostatic pressing or other processes;
[0017] Among them, the static pressure molding pressure is ≥10MPa and the temperature is ≥-40℃.
[0018] The best combination of metal powders involved in the present invention is copper powder or mixed powder of copper powder and aluminum powder.
[0019] Compared with the prior art, the present invention provides a novel method for preparing an antifouling electrode, wherein metal powder, antifouling agent powder and polymer material powder are uniformly mixed to prepare plastic antifouling powder, and then the antifouling powder is filled into foamed metal (foamed metal is an optional structure, and an antifouling electrode can be prepared by an isostatic forming process without using foamed metal, but the strength of the antifouling electrode is relatively low) to prepare an antifouling electrode precursor, and finally an antifouling electrode with excellent mechanical properties and high antifouling ion release efficiency is obtained by static pressing and other processes, and a variety of antifouling agents can be efficiently and stably released in a seawater environment, and the release efficiency is improved by more than 50% relative to conventional antifouling copper electrodes; the preparation process principle is scientific and reliable, and the prepared antifouling electrode has excellent antifouling effect, meeting the antifouling needs of various underwater marine facilities and equipment. Description of the drawings:
[0020] Figure 1 It is a schematic diagram of a coupling current curve of a galvanic corrosion test involved in the present invention. Specific implementation method:
[0021] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0022] Embodiment 1:
[0023] The specific process of the antifouling electrode preparation method involved in this embodiment is as follows:
[0024] (1) Under room temperature, 50 g of copper powder and 50 g of cuprous oxide powder were placed in a blender, mixed, and stirred evenly to obtain an antifouling powder;
[0025] (2) pouring antifouling powder into a mold;
[0026] (3) Cold isostatic pressing process: A force of 10 MPa was uniformly applied and the pressure was maintained for 2 h to obtain the antifouling electrode A1.
[0027] Embodiment 2:
[0028] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Embodiment 1, except that a force of 100 MPa is uniformly applied through a cold isostatic pressing process to obtain the antifouling electrode A2.
[0029] Embodiment 3:
[0030] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 1, except that a cold isostatic pressing process is provided to uniformly apply a force of 200 MPa to obtain the antifouling electrode A3.
[0031] Embodiment 4:
[0032] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 3, except that the mass of the copper powder is 70 g, the mass of the cuprous oxide powder is 30 g, and the obtained antifouling electrode is A4.
[0033] Embodiment 5:
[0034] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 3, except that the mass of the copper powder is 90 g, the mass of the cuprous oxide powder is 10 g, and the obtained antifouling electrode is A5.
[0035] Embodiment 6:
[0036] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 3, except that the mass of the copper powder is 100 g, the mass of the cuprous oxide powder is 0 g, and the obtained antifouling electrode is A6.
[0037] Embodiment 7:
[0038] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 4, except that 30g of cuprous oxide powder is replaced by a mixture of 20g of cuprous oxide powder and 10g of Econea powder, and the obtained antifouling electrode is A7.
[0039] Embodiment 8:
[0040] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 7, except that the antifouling powder is replaced with a mixture of 100g of antifouling powder and 10g of polyethylene powder to obtain the antifouling electrode A8.
[0041] Embodiment 9:
[0042] The specific process of the antifouling electrode preparation method involved in this embodiment is the same as that of Example 8, except that the plastic antifouling powder (a mixture of 70g copper powder, 20g cuprous oxide powder, 10g Econea powder and 10g polyethylene powder) is evenly filled into a 20PPi foam copper frame to obtain an antifouling electrode precursor, and then the antifouling electrode precursor is placed in a mold, the temperature is set to 120°C, and an antifouling electrode is prepared by hot isostatic pressing, which is recorded as A9.
[0043] Comparative Example 1:
[0044] The antifouling electrode prepared by using copper plate, as a comparative example, was recorded as D1, and was subjected to galvanic corrosion test and tensile property test with A1-A9 respectively;
[0045] Galvanic corrosion test The galvanic corrosion test was carried out with reference to GB / T 15748-2013 Galvanic corrosion test method for marine metal materials. The test solution was natural seawater (10L). The test period was 3 days. The coupling current and potential information were measured in real time by a galvanic corrosion measuring instrument. After the test, the test solution was dissolved by hydrochloric acid. The copper concentration in the water sample was detected by an inductively coupled plasma mass spectrometer according to HY / T 147.1-2013 to analyze the release efficiency of the anti-fouling electrode.
[0046] The coupling current under different antifouling electrodes is as follows Figure 1 As shown, it can be seen from the curves of A3-A6 that the antifouling ion release efficiency of the antifouling electrode obtained is different based on the different ratios of copper powder and cuprous oxide powder, among which the antifouling electrode obtained by the ratio of A4 has the highest release efficiency; it can be seen from the curves of A4, A7 and A8 that the addition of Econea powder and polyethylene powder has no significant effect on the release efficiency of antifouling ions, but the diffusion of Econea powder enhances the antifouling effect of the antifouling electrode; it can be seen from the curves of A4 and A9 that the release efficiency of antifouling ions of the antifouling electrode prepared by the hot pressing molding process is slightly improved; from the comparison of D1 and A4-A9, it can be seen that the release efficiency of antifouling ions of A4-A9 is significantly higher;
[0047] According to the anti-fouling electrode galvanic test water sample detection record form:
[0048]
[0049] It can be seen that while the release effect of the antifouling ions of the antifouling electrodes A3-A9 is significantly improved, the release effect of the antifouling ions can be further improved by changing the ratio of the antifouling ions.
[0050] The tensile properties test refers to "GB / T 228.1-2021 Tensile Test of Metal Materials". The mechanical properties (tensile strength and elongation at break) of Examples A1-4, A7 and A9 are tested at a tensile rate of 10 mm / min. The results are shown in the following table:
[0051]
[0052]
[0053] It can be seen that the mechanical properties of A1-A3 gradually increase with the increase of the pressure of the isostatic forming process; the mechanical properties of A3, A4 and A7 are not much different, and A8 uses foam metal as the frame, which greatly improves the mechanical properties of the anti-fouling electrode.
[0054] In summary, the antifouling electrode preparation method can be used to prepare an antifouling electrode with excellent mechanical properties and conductive properties that can stably, reliably and efficiently release a variety of antifouling ions.
Claims
1. A novel method for preparing an efficient antifouling electrode, characterized in that: The specific process is as follows: (1) mixing metal powder and antifouling agent powder uniformly to obtain antifouling powder; (2) mixing the antifouling powder and the polymer material powder uniformly to obtain a plastic antifouling powder; (3) filling the plastic antifouling powder into the foam metal to obtain an antifouling electrode precursor; (4) Pressing the antifouling electrode precursor into an antifouling electrode.
2. A novel high-efficiency antifouling electrode preparation method according to claim 1, characterized in that: The metal powder in step (1) is one or more metal powders that can be corroded and dissolved in seawater, including copper powder, aluminum powder, and iron powder.
3. A novel high-efficiency antifouling electrode preparation method according to claim 2, characterized in that: The antifouling agent powder in step (1) is one or more of organic and inorganic antifouling agents, including cuprous oxide, cuprous thiocyanate, zinc oxide, copper sulfate, copper cyclohexaneate, acid copper, organic tin, DDT, Econea, zinc pyrithione, and pyridine triphenylborane.
4. A novel high-efficiency antifouling electrode preparation method according to claim 3, characterized in that: The weight ratio of the antifouling agent powder to the metal powder in step (1) is 0-2:
1.
5. A novel high-efficiency antifouling electrode preparation method according to claim 1, characterized in that: The polymer material powder in step (2) is one or more materials that can melt at a set temperature, including polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyoxymethylene, polycarbonate, polyamide, acrylic plastics, polyolefins and copolymers thereof, polysulfones, polyphenylene ethers, and chlorinated polyethers.
6. A novel high-efficiency antifouling electrode preparation method according to claim 5, characterized in that: The weight ratio of the polymer material powder to the antifouling powder in step (2) is 0-0.2:
1.
7. A novel high-efficiency antifouling electrode preparation method according to claim 1, characterized in that: The foam metal in step (3) includes one or more of foam copper, foam nickel, and foam aluminum.
8. A novel high-efficiency antifouling electrode preparation method according to claim 1, characterized in that: Step (4) presses the antifouling electrode precursor into an antifouling electrode through an isostatic pressing process.
9. A novel high-efficiency antifouling electrode preparation method according to claim 8, characterized in that: The pressure of isostatic pressing is ≥10MPa and the temperature is ≥-40℃.
10. A novel high-efficiency antifouling electrode preparation method according to any one of claims 2 to 4, characterized in that: The metal powder is copper powder or a mixed powder of copper powder and aluminum powder.
Citation Information
Patent Citations
Power-free long-life self-driven anti-fouling device for ship seawater box environment
CN113481511A