Brass welding material for welding and preparation method thereof

By adjusting the composition ratio and process flow of brass welding materials, an optimized microstructure is formed, which solves the problems of poor welding performance and poor corrosion resistance, and achieves the close color of the weld and the parent body, excellent welding performance and corrosion resistance. Effect.

CN119077217APending Publication Date: 2024-12-06JINTIAN COPPER GROUP CORP NINGBO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411438475.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the welding process, existing brass welding materials have problems such as poor welding performance, poor corrosion resistance, large color contrast, and easy to have pores, slag inclusion and cracks, which affect the beauty and quality of the jewelry.

Method used

By adjusting the composition ratio of brass welding materials, the Cu content is increased to 65-70 wt%, and elements such as Sn, Si, P are added to control the proportion and grain size of the β phase, and the continuous pulling and retreating process and step annealing process are adopted. Form an optimized microstructure to improve welding performance and corrosion resistance.

Benefits of technology

The weld is close to the color of the brass parent body, excellent welding performance, corrosion resistance and high-temperature oxidation resistance are improved, reducing the occurrence of pores and cracks, and improving the overall quality of welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077217A_ABST
    Figure CN119077217A_ABST
Patent Text Reader

Abstract

The invention discloses a brass welding material for welding and a preparation method thereof. The brass welding material comprises the following components in percentage by mass: 65 to 70 weight percent of Cu, 0.2 to 0.8 weight percent of Sn, 0.05 to 0.6 weight percent of Si, 0.002 to 0.01 weight percent of P, 0.01 to 0.10 weight percent of Fe, less than or equal to 0.01 weight percent of Pb, Bi and S, and the balance of Zn and inevitable impurities. The brass welding material has good welding performance and high-temperature oxidation resistance, and the color of a welded weld joint is close to that of a brass matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of brass, and in particular relates to a brass welding material for welding and a preparation method thereof. Background Art

[0002] Brass is a binary alloy composed of Cu and Zn elements. Its room temperature structure changes with the change of Zn content. According to the Cu-Zn phase diagram, there are two room temperature structures of processed brass: brass with a Zn content below 35% has a microstructure composed of only α phase at room temperature, which is called α brass (single-phase brass); brass with a Zn content in the range of 36-46% has a microstructure composed of (α+β) two phases at room temperature, which is called (α+β) brass (two-phase brass).

[0003] Brass is golden in color and its price is much lower than gold. Therefore, it is widely used in the production of various artistic decorations, and welding is often required in the production process. When welding jewelry, the welding material directly participates in a series of chemical metallurgical reactions in the welding process, which determines the composition, structure, performance and defect formation of the weld metal. At present, there are few brass welding materials specially used for jewelry and welding on the market. At present, most brass jewelry welding uses ordinary brass welding materials, which often have poor welding performance, large color contrast with the parent brass, poor corrosion resistance, and problems such as pores, slag inclusions, and cracks, which affect the beauty of the jewelry welding.

[0004] The invention patent application with publication number CN109434318A discloses a tin brass alloy solder, which contains: 61.5-63wt.% Cu, 0.7-1.0wt.% Sn, 0.4-0.8wt.% Si, 0.02-0.2wt.% Ni, 0.02-0.2wt.% Al, 0.02-0.15wt.% As, 0.02-0.2wt.% Ti, and the rest is Zn and unavoidable impurities, wherein the total content of Cu and Zn is greater than 97.0wt.%. The zinc content in the alloy disclosed in the patent application is still relatively high, and the evaporation of zinc during the welding process can still affect the welding performance.

[0005] The invention patent application with publication number CN115354188A discloses an easy-to-weld brass, the mass percentage composition of which is Cu: 60-63wt%, Pb: 0.1-0.5wt%, Al≤0.05wt%, Bi≤0.008wt%, Si: 0.02-0.10%, Zr: 0.008-0.06%, and the balance is Zn and unavoidable impurities. The brass of the present invention limits the content of the main element Cu of brass and the content of impurity elements Al and Bi that affect the welding performance of the material, and at the same time adds beneficial elements Si and Zr that improve the welding performance of brass, thereby realizing the matrix phase of α phase and β phase and controlling the area proportion of β phase. The brass alloy disclosed in the invention patent is easily oxidized and discolored after welding.

[0006] Since zinc has a low boiling point of only 907°C, it is very easy to evaporate during welding. The large amount of evaporation of zinc leads to a decrease in the mechanical properties and corrosion resistance of the weld. Brass has good thermal conductivity, the welding molten pool solidifies quickly, and the gas in the liquid molten pool floats for a short time, so it has no time to escape and form pores. The presence of harmful impurity elements in brass easily forms low-melting eutectics and brittle compounds during welding, and thermal cracks are prone to occur at the weld. Under the action of welding heat, the grains grow severely, the oxidation of useful alloy elements and various brittle low-melting eutectics appear at the grain boundaries or produce brittle phases, which significantly reduce the plasticity and corrosion resistance of the metal at the weld.

[0007] Therefore, in order to solve the above problems, it is necessary to improve the existing ordinary brass welding materials and propose a brass welding material suitable for welding jewelry. The weld of the jewelry welded by the brass welding material is close in color to the brass matrix, and the corrosion resistance of the weld is better than that of ordinary brass welding materials. Summary of the invention

[0008] The invention provides a brass welding material for welding. The brass welding material has good welding performance, corrosion resistance and high-temperature oxidation resistance, and the color of the weld after welding is close to that of the brass matrix.

[0009] The invention provides a brass welding material for welding. The mass percentages of the components of the brass welding material are Cu: 65-70wt%, Sn: 0.2-0.8wt%, Si: 0.05-0.6wt%, P: 0.002-0.01wt%, Fe: 0.01-0.10wt%, Pb+Bi+S≤0.01wt%, and the balance is Zn and inevitable impurities.

[0010] The functions of the elements provided by the present invention are described as follows:

[0011] Cu: The Cu content affects the ratio of α phase and β phase in the brass structure, and further affects the corrosion resistance of brass. When the Cu content is lower than 64.0wt%, it can be seen from the Cu-Zn phase diagram that a certain proportion of β phase will appear in the original single-phase brass structure; when the Cu content exceeds 64%, the room temperature structure of brass is a single-phase α phase structure. Considering that Sn and Si elements are added to the brass of the present invention, because their zinc equivalent coefficients are +4 and +10 respectively, and the values ​​are relatively large, the proportion of β phase in the brass microstructure can be significantly increased. In order to control the appropriate phase ratio, the Cu content of the brass of the present invention is in the range of 65-70wt%.

[0012] Si: The role of Si is to form a dense SiO2 film on the surface of the molten pool after the brass is melted, which hinders the evaporation of Zn and makes the metal fusion of the welding part round and smooth. The oxide film can prevent the dissolution of hydrogen and produce pores. If the Si content is too low, the effect of improving the roundness of the weld is poor, and it is easy to cause pores in the weld. However, the Si content should not be too high. When the Si content exceeds 0.6%, on the one hand, the thickness of the SiO2 film will increase, affecting the discharge of gas during welding, and more pores will appear; on the other hand, since the zinc equivalent coefficient of Si is +10, the addition of Si to brass can significantly increase the β phase. Since the β phase is less corrosion-resistant than the α phase, the corrosion resistance of brass decreases, and the brittleness of brass is increased, making the brass welding material difficult to process. Therefore, the content of Si element added to the brass of the present invention should be controlled at 0.05-0.6wt%.

[0013] Sn: After adding Sn, the wettability of brass welding materials is improved, and it can wet the surface of the metal being welded well, making the weld smooth and round. Sn can improve the strength and corrosion resistance of the weld. When the Sn content is less than 0.2wt%, the effect of improving the wettability of brass welding materials is poor. When the Sn content exceeds 0.8wt%, the proportion of β phase in the brass structure increases, and the anti-dezincification performance of the welding material decreases.

[0014] P: Brass has high thermal conductivity and the crystallization speed of weld metal is very fast. Under such conditions, it is difficult for hydrogen to diffuse and escape and bubbles to float up. Pores are often formed before they have time to escape and float up. Adding a deoxidizer to the welding material can reduce the generation of pores. In the present invention, the main function of P is to enhance the deoxidation ability of the weld, improve the fluidity of the molten pool metal, and reduce the generation of pores. However, if the P content is too high, it will have a negative impact on the processing performance of brass, and if the content is too low, the deoxidation effect is poor. Therefore, the content of P element added to the brass of the present invention should be controlled at 0.002-0.01wt%.

[0015] Fe: A trace amount of Fe in brass can increase the recrystallization temperature and inhibit the growth of α phase and β phase. Therefore, the Fe content of the brass of the present invention is controlled at 0.01-0.10wt%.

[0016] Pb+Bi+S: The solubility of Pb, Bi and S in α brass is extremely low. When the sum of the contents of Pb, Bi and S in single-phase brass such as H65 exceeds 0.01wt%, low-melting-point eutectics Cu+Pb (melting point 327°C), Cu+Bi (melting point 270°C) and Cu+S (melting point 645°C) are generated during the crystallization of the molten pool. These eutectics are distributed in a network-like manner between the dendrites or at the grain boundaries of the weld metal. When the weld is at a high temperature, thermal cracks will occur on the weld.

[0017] Preferably, the contents of Cu, Sn and Si satisfy the following relationship:

[0018] M Cu -(M Sn ×4+M Si ×10)≥63wt%

[0019] Among them, M Cu is the content of Cu, M Si is the content of Si, M Sn is the Sn content.

[0020] When the Cu content and Sn, Si content meet: M Cu -(M Sn ×4+M Si ×10)≥63wt%, the corrosion resistance of the brass welding material is better, because the zinc equivalent coefficients of Sn and Si are relatively high, which are +4 and +10 respectively. Every increase of 0.1% Sn is equivalent to an increase of 0.4wt% Zn, and every increase of 0.1% Si is equivalent to an increase of 1wt% Zn. The Cu content affects the corrosion resistance of brass, and the corrosion resistance of brass decreases with the decrease of Cu content. Therefore, the present invention maintains the Cu content at a higher level on the basis of avoiding the introduction of excessive impurities during the welding process through the above-mentioned relationship, so that the corrosion resistance of the brass welding material is better. The contents of Cu, Sn and Si mentioned in the present invention are mass percentage contents.

[0021] Preferably, the brass welding material further comprises In, and the mass percentage of In is 0.003-0.018wt%. The chemical properties of In are very stable, and In and Sn form an intermetallic compound InSn, which has a more stable chemical property. Compared with the simple addition of Sn, the corrosion resistance of the weld can be further improved; in addition, the brass welding material with a trace amount of In element added, the weld formed by welding is not easy to crack, because a trace amount of In can improve the toughness of the weld. Therefore, under a higher Cu content, adding an appropriate amount of In can improve the welding performance. In the present invention, the addition amount of In is 0.003-0.018wt%, and the strength of the weld will decrease when the In content exceeds 0.018wt%.

[0022] Preferably, the structure of the brass welding material for welding includes α phase and β phase, the area of ​​the β phase accounts for less than 5%, and the size of the α phase is 0.003-0.01 mm. The present invention controls the size of the α phase and the area of ​​the β phase, so that the brass welding material provided by the present invention has good corrosion resistance and oxidation resistance.

[0023] Preferably, the thermal properties of the brass solder for welding are: a melting point range of 900-940°C, a thermal conductivity of 118-125w / (m·k), and a linear expansion coefficient of 19.2-20.4μm / (m·k) at 20-300°C. The brass solder provided by the present invention has a lower melting point range and is relatively easy to heat and cool, and is combined with a higher thermal conductivity and a suitable linear expansion coefficient, which is conducive to the welding process.

[0024] Preferably, the maximum dezincification layer depth of the brass welding material is ≤50 μm, and the high temperature oxidation resistance should meet the following requirements: no oxidation discoloration after baking at 250°C for 3 minutes. The brass welding material provided by the present invention has good corrosion resistance and oxidation resistance, and is not easily affected by the external environment.

[0025] The present invention also provides a method for preparing the brass welding material for welding, and the process flow of the preparation method comprises: smelting→horizontal continuous casting→coil drawing→annealing→continuous drawing and annealing;

[0026] Wherein, the brass welding material for welding is prepared and smelted according to the mass percentage of each component;

[0027] The continuous pulling and continuous retreating includes large pulling and continuous retreating, medium pulling and continuous retreating and small pulling and continuous retreating;

[0028] The processing rate of the large-scale continuous drawing and annealing is 55-70%, the drawing speed is 2-10 mm / s, and the annealing current is 800-2000 A;

[0029] The processing rate of the intermediate drawing and annealing is 65-90%, the drawing speed is 3-12 mm / s, and the annealing current is 500-800 A;

[0030] The processing rate of the small continuous drawing and annealing is 60-90%, the stretching speed is 5-20 mm / s, and the annealing current is 60-300A.

[0031] The continuous drawing and annealing provided by the present invention is to anneal the copper wire online while stretching it. Due to the skin effect, in the continuous drawing and annealing process, the temperature of the surface of the billet is higher than the temperature of the core, which easily causes inconsistent grain size. The present invention controls the annealing current, processing rate and drawing speed of three consecutive online annealings, so that the billet grains are finally small and uniform.

[0032] The present invention controls the processing rate, stretching speed and annealing current of large-size billets so that the grain sizes of the surface and the core of the billet are close at a higher annealing temperature and an extremely short annealing time, and the grains do not have time to grow in the extremely short annealing time.

[0033] The present invention controls the processing rate, stretching speed and annealing current of the intermediate drawing and annealing process so that the grain sizes of the surface and the core of the billet with reduced diameter are further approached at the second highest annealing temperature and the extremely short annealing time, and the grains do not have time to grow in the extremely short annealing time.

[0034] The present invention controls the processing rate, stretching speed and annealing current of the small continuous drawing process so that the grain sizes of the surface and the core of the billet with a further reduced diameter are closest at a lower annealing temperature and an extremely short annealing time, and the grains do not have time to grow in the extremely short annealing time.

[0035] Compared with the existing one-step continuous drawing and annealing process, the three-step continuous drawing and annealing process provided by the present invention can produce a structure with a smaller grain size and more uniformity, and the parameters of the preparation process are easier to control.

[0036] Preferably, the annealing voltage of the large continuous annealing is 20-80 V, the annealing voltage of the medium continuous annealing is 30-150 V, and the annealing voltage of the small continuous annealing is 50-160 V. By controlling the annealing voltage of each pass, the corresponding annealing current is ensured to have a high stability and a suitable annealing temperature.

[0037] Preferably, before continuous drawing and retreating, the specification of the blank is Φ5.5-8.5mm.

[0038] Preferably, the emulsion concentration of the large-scale continuous drawing is 3-7%, the emulsion concentration of the medium-scale continuous drawing is 5-9%, and the emulsion concentration of the small-scale continuous drawing is 6-12%.

[0039] Preferably, the annealing comprises a gradient three-stage annealing;

[0040] Among them, the annealing temperature of the first stage is 400-440°C, and the holding time is 180-240min;

[0041] The annealing temperature in the second stage is 480-520°C and the holding time is 90-210min;

[0042] The annealing temperature of the third stage is 580-620°C, and the holding time is 45-90 minutes.

[0043] Furthermore, after the gradient three-stage annealing, the billet is air-cooled to 250-300°C and finally water-cooled to 60°C to room temperature.

[0044] The purpose of the step annealing of the present invention is to firstly heat-hold the alloy in the lower limit range of the recrystallization temperature for a long time to start slow recrystallization, so as to obtain fine grains, and then continue to increase the temperature to the middle limit range of the recrystallization temperature for heat-holding, so as to allow the fine recrystallized grains formed in the first stage to grow slowly, and finally increase the temperature to the upper limit range of the recrystallization temperature for heat-holding, so as to promote the further growth of the grains to form equiaxed crystals in a relatively short time, and completely remove the as-cast structure of the horizontal continuous casting, so as to avoid the failure to obtain a uniform recrystallized structure during the subsequent continuous drawing and annealing process during online annealing; at the same time, the work hardening is completely eliminated, so that the performance of the billet is completely softened, and the completely softened billet can be stretched to the required specifications through continuous drawing and annealing, so as to avoid the failure to obtain a billet of the required specifications through continuous drawing and annealing due to the initial billet being too hard.

[0045] Further preferably, annealing is performed in a strong convection hood-type bright annealing furnace, using a mixture of H2 and N2 as a protective gas, with the volume proportion of H2 being ≥75%, and the purpose of gas protection is to ensure that the surface of the wire is not oxidized. In order to improve the uniformity of annealing performance, a step-type annealing process is adopted, firstly, the temperature in the hood furnace is raised from room temperature to 400-440°C after 40-60 minutes, and the first insulation is carried out for 150-240 minutes; then the temperature in the hood furnace is raised to 480-520°C after 15-25 minutes, and the second insulation is carried out for 90-210 minutes; then the temperature in the hood furnace is raised to 580-620°C after 15-25 minutes, and the third insulation is carried out for 45-90 minutes; after the third insulation is completed, the cooling hood is replaced with air cooling to 250-300°C, and finally water is added for water cooling to 60°C ~ room temperature before being taken out of the furnace.

[0046] Preferably, the smelting process is: mixing and melting the raw materials according to the mass percentage of each component of the brass welding material for welding, then adding a slag cleaning agent to stir and remove the slag, and then adding a mixed rare earth element, wherein the mixed rare earth element mainly consists of Ce, La, Nd and Pr;

[0047] The raw materials include electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy and copper-phosphorus master alloy, and the order of adding materials is electrolytic copper→copper-silicon master alloy and copper-iron master alloy→zinc ingot→tin ingot→copper-phosphorus master alloy.

[0048] The smelting process provided by the invention comprises the following steps: electrolytic copper, zinc ingot, tin ingot, copper-silicon master alloy (containing Si 20wt%), copper-iron master alloy (containing Fe 5wt%) and copper-phosphorus master alloy (containing P 14wt%) are added into a smelting furnace according to the required alloy component ratio and the order of adding materials (electrolytic copper→copper-silicon master alloy and copper-iron master alloy→zinc ingot→tin ingot→copper-phosphorus master alloy) to heat and melt; after the components meet the requirements, a slag remover is added to stir and remove the slag; then, a mixed rare earth mainly consisting of Ce, La, Nd and Pr is added to be fully stirred; the added amount is 0.006-0.02wt%; the rare earth metal has high activity; during alloy smelting, it is very easy to react with Pb and Bi to form high melting point stable compounds; and react with S to form sulfides; the density of these compounds is lower than that of copper, so they are easy to float and be removed from the copper liquid; finally, the mixture is transferred into a heat preservation furnace through a submerged liquid transfer mode for heat preservation; and the temperature is controlled at 1040-1070°C.

[0049] Preferably, the temperature of the horizontal continuous casting is 1040-1070°C, the pulling pitch is 4-15mm, the pulling time is 0.05-0.6s, the pulling stop time is 0.01-0.2s, the reverse thrust pitch is 0.4-3mm, and the reverse thrust time is 0.02-0.3s.

[0050] Further, the horizontal continuous casting process provided by the present invention is as follows: the molten copper is continuously led out horizontally from the holding furnace by the crystallizer, the rod billet specification is Φ8-12mm, the casting temperature is 1040-1070℃, the cooling water inlet temperature is 15-32℃, the outlet temperature is 25-42℃, the traction action performs the "pull-stop-reverse push-pull" steps, and adopts a low-speed, high-frequency process, that is, while reducing the traction speed, the traction pitch is reduced, and the traction parameters are: traction pitch 4-15mm, traction time 0.05-0.6s, pull stop time 0.01-0.2s, reverse push pitch 0.4-3mm, and reverse push time 0.02-0.3s. Low-speed traction is equivalent to enhancing the cooling strength of the billet. When the molten copper is crystallized at a high frequency, the effect of vibrating and breaking dendrites is more obvious, and a billet with dense as-cast structure and small intracrystalline segregation can be obtained.

[0051] Preferably, the coiling process is: first stretching→first peeling→second stretching→second peeling;

[0052] Among them, the processing rate of the first extension is 20-30%, the peeling amount of the first peeling is 0.2-0.3mm, the processing rate of the second extension is 10-25%, and the peeling amount of the second peeling is 0.15-0.25mm.

[0053] Before the first peeling, the horizontal continuous casting rod blank is stretched at a processing rate of 20-30% to fully harden the surface of the rod blank, improve the roundness of the wire blank, and obtain a uniform peeling amount. The first peeling amount is controlled at 0.2-0.3mm. After the first peeling, it is stretched at a processing rate of 10-25%, and then the second peeling is carried out. The second peeling amount is controlled at 0.15-0.25mm. After two peelings, casting defects such as crystal lines, zinc spots, small cracks, etc. on the surface of the rod blank are completely eliminated.

[0054] Preferably, the total processing rate of the coiling is 40-53%, and the total stripping amount is 0.3-0.5 mm. The present invention uses coiling to continuously pull the Φ8-12 mm horizontal continuous casting rod to Φ5.5-8.5 mm in multiple passes.

[0055] Compared with the prior art, the present invention has the following beneficial effects:

[0056] The present invention provides a higher content of Cu to reduce the content of Zn, thereby improving welding performance. At the same time, since the addition of Sn and Si with high zinc equivalent leads to an increase in the proportion of β phase, the present invention can also reduce the proportion of β phase by increasing the Cu content, inhibiting the influence of Sn and Si on the phase structure, so that the brass structure provided by the present invention is a single α phase structure or contains only a small amount of β phase, thereby improving the corrosion resistance and high temperature oxidation resistance of brass, and then the color of the weld after welding is close to that of the brass matrix; due to the high content of Cu provided by the present invention, the fluidity of the alloy is enhanced during the welding process, so that it is easier to introduce oxide impurities during the welding process. In order to avoid introducing too many impurities, the present invention removes them by adding appropriate amounts of Sn, Si and P, thereby improving welding performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a metallographic structure photo of Example 1 of the present invention;

[0058] Figure 2 This is a metallographic structure photograph of Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0059] The present invention is further described in detail below with reference to the accompanying drawings.

[0060] The present invention provides 4 embodiments and 3 comparative examples, and the specific components are shown in Table 1.

[0061] Example 1

[0062] A brass welding material for welding, with a specification of Φ0.6mm, is produced as follows:

[0063] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, and copper-phosphorus master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag. Then, a mixed rare earth is added and stirred sufficiently. The addition amount is 0.008wt%. Finally, the mixture is transferred into a holding furnace for insulation through a submerged liquid transfer method. The temperature is controlled at 1050-1060°C.

[0064] (2) Horizontal continuous casting: the rod billet specification is Φ9.8mm, the casting temperature is 1050-1060℃, the cooling water inlet temperature is 28℃, the outlet temperature is 36℃, the traction pitch is 8mm, the traction time is 0.5s, the pause time is 0.08s, the reverse thrust pitch is 1mm, and the reverse thrust time is 0.1s.

[0065] (3) Coil pulling: The Φ9.8mm billet is first pulled to Φ7.22mm in multiple passes, with a processing rate of 45.7%. Two peeling passes are required in the middle, and the total peeling amount is 0.42mm. The specific processing technology is: in the first pass, the Φ9.8mm billet is coiled to Φ8.4mm with a processing rate of 26.5%, and then peeled to Φ8.16mm, with a peeling amount of 0.24mm; in the second pass, the Φ8.16mm billet is coiled to Φ7.4mm, and then peeled to Φ7.22mm, with a peeling amount of 0.18mm.

[0066] (4) Annealing: The Φ7.22mm wire billet is step-annealed in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 400°C in 45 minutes and kept at this temperature for 210 minutes; then, the temperature in the bell-type furnace is raised to 490°C in 20 minutes and kept at this temperature for 150 minutes; then, the temperature in the bell-type furnace is raised to 600°C in 25 minutes and kept at this temperature for 60 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 270°C. Finally, water is added for water cooling to 60°C and then the wire is taken out of the furnace at room temperature.

[0067] (5) Continuous pulling and retreating:

[0068] a. Large drawing and annealing: After bell-type furnace annealing, the Φ7.22mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ4.1mm. The processing rate is 67.8%, the stretching speed is 5mm / s, the annealing voltage is 32V, the annealing current is 1180A, and the emulsion concentration is 5.2%.

[0069] b. Intermediate drawing and continuous annealing: The Φ4.1mm wire billet is stretched to Φ1.8mm through intermediate drawing and continuous annealing, the processing rate is controlled at 80.7%, the stretching speed is 7mm / s, the annealing voltage is 105V, the annealing current is 280A, and the emulsion concentration is 7.3%.

[0070] c. Small continuous drawing and annealing: Φ1.8mm is stretched through the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ0.6mm, with a processing rate of 88.9%.

[0071] The stretching speed was 10 mm / s, the annealing voltage was 60 V, the annealing current was 122 A, the coolant temperature was 30° C., and the emulsion concentration was 8.4%.

[0072] (6) Inspect the packaging.

[0073] Example 2

[0074] A brass welding material for welding, with a specification of Φ0.8mm, is produced as follows:

[0075] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, and copper-phosphorus master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag. Then, a mixed rare earth is added and stirred sufficiently. The addition amount is 0.01wt%. Finally, the mixture is transferred into a holding furnace for insulation through a submerged liquid transfer method. The temperature is controlled at 1050-1060°C.

[0076] (2) Horizontal continuous casting: the rod billet specification is Φ10.8mm, the casting temperature is 1055-1065℃, the cooling water inlet temperature is 24℃, the water outlet temperature is 33℃, the traction pitch is 6mm, the traction time is 0.6s, the pause time is 0.1s, the reverse thrust pitch is 1.2mm, and the reverse thrust time is 0.15s.

[0077] (3) Coil pulling: The Φ10.8mm billet is first pulled in multiple passes to Φ7.45mm, with a processing rate of 52.4%. Two peeling passes are required in the middle, and the total peeling amount is 0.36mm. The specific processing technology is: in the first pass, the Φ10.8mm billet is coiled to Φ9.2mm with a processing rate of 27.4%, and then peeled to Φ9mm, with a peeling amount of 0.20mm; in the second pass, the Φ9mm billet is coiled to Φ7.8mm with a processing rate of 24.9%, and then peeled to Φ7.64mm, with a peeling amount of 0.16mm.

[0078] (4) Annealing: The Φ7.64mm wire billet is step-annealed in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 440°C over 60 minutes and kept at this temperature for 180 minutes; then, the temperature in the bell-type furnace is raised to 500°C over 20 minutes and kept at this temperature for 120 minutes; then, the temperature in the bell-type furnace is raised to 580°C over 25 minutes and kept at this temperature for 60 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 250°C. Finally, water is added for water cooling to 60°C and then the wire is taken out of the furnace at room temperature.

[0079] (5) Continuous pulling and retreating:

[0080] a. Large drawing and annealing: After bell-type furnace annealing, the Φ7.64mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ4.5mm. The processing rate is 65.3%, the stretching speed is 4.8mm / s, the annealing voltage is 38V, the annealing current is 1240A, and the emulsion concentration is 5.6%.

[0081] b. Intermediate drawing and continuous annealing: The Φ4.5mm wire billet is stretched to Φ2.2mm through intermediate drawing and continuous annealing, the processing rate is controlled at 76.1%, the stretching speed is 6mm / s, the annealing voltage is 120V, the annealing current is 330A, and the emulsion concentration is 6.9%.

[0082] c. Small continuous drawing and annealing: Φ2.2mm is stretched through the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ0.8mm, the processing rate is 86.7%, the stretching speed is 9mm / s, the annealing voltage is 70V, the annealing current is 130A, and the emulsion concentration is 8%.

[0083] (6) Inspect the packaging.

[0084] Example 3

[0085] A brass welding material for welding, with a specification of Φ1.2mm, is produced as follows:

[0086] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, and copper-phosphorus master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag. Then, a mixed rare earth is added and stirred sufficiently. The addition amount is 0.014wt%. Finally, the mixture is transferred into a holding furnace through a submerged liquid transfer method to be kept warm. The temperature is controlled at 1060-1070°C.

[0087] (2) Horizontal continuous casting: the rod billet specification is Φ12mm, the casting temperature is 1060-1070℃, the cooling water inlet temperature is 18℃, the water outlet temperature is 27℃, the traction pitch is 6mm, the traction time is 1.0s, the pause time is 0.12s, the reverse thrust pitch is 1.0mm, and the reverse thrust time is 0.12s.

[0088] (3) Coil pulling: The Φ12mm billet is first pulled in multiple passes to Φ8.8mm, with a processing rate of 46.2%. Two peeling passes are required in the middle, and the total peeling amount is 0.45mm. The specific processing technology is: in the first pass, the Φ12mm billet is coiled to Φ10.2mm with a processing rate of 27.4%, and then peeled to Φ9.95mm, with a peeling amount of 0.25mm; in the second pass, the Φ9.95mm billet is coiled to Φ9mm with a processing rate of 18.2%, and then peeled to Φ8.8mm, with a peeling amount of 0.20mm.

[0089] (4) Annealing: The Φ8.8 mm wire billet is subjected to step annealing in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 440°C over 60 minutes and kept at this temperature for 150 minutes; then, the temperature in the bell-type furnace is raised to 510°C over 20 minutes and kept at this temperature for 150 minutes; then, the temperature in the bell-type furnace is raised to 620°C over 25 minutes and kept at this temperature for 45 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 240°C. Finally, water is added for water cooling to 60°C and then the wire billet is taken out of the furnace at room temperature.

[0090] (5) Continuous pulling and retreating:

[0091] a. Large drawing and annealing: After bell-type furnace annealing, the Φ8.8mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ5.6mm. The processing rate is 59.5%, the stretching speed is 4mm / s, the annealing voltage is 50V, the annealing current is 1320A, and the emulsion concentration is 5%.

[0092] b. Intermediate drawing and continuous annealing: The Φ5.6mm wire billet is stretched to Φ3.2mm through intermediate drawing and continuous annealing, the processing rate is controlled at 67.3%, the stretching speed is 5.5mm / s, the annealing voltage is 140V, the annealing current is 380A, and the emulsion concentration is 6%.

[0093] c. Small continuous drawing and annealing: Φ3.2mm is stretched by the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ1.2mm, with a processing rate of 85.9%.

[0094] The stretching speed was 7 mm / s, the annealing voltage was 92 V, the annealing current was 160 A, and the emulsion concentration was 8.5%.

[0095] (6) Inspect the packaging.

[0096] Example 4

[0097] A brass welding material for welding, with a specification of Φ0.6mm, is produced as follows:

[0098] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, copper-phosphorus master alloy, and copper-indium master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag, and then mixed rare earth is added and fully stirred in an amount of 0.008wt%. Finally, the mixture is transferred into a holding furnace for insulation by a submerged liquid transfer method, and the temperature is controlled at 1050-1060°C.

[0099] (2) Horizontal continuous casting: the rod billet specification is Φ9.8mm, the casting temperature is 1050-1060℃, the cooling water inlet temperature is 28℃, the outlet temperature is 36℃, the traction pitch is 8mm, the traction time is 0.5s, the pause time is 0.08s, the reverse thrust pitch is 1mm, and the reverse thrust time is 0.1s.

[0100] (3) Coil pulling: The Φ9.8mm billet is first pulled in multiple passes to Φ7.22mm, with a processing rate of 45.7%. Two peeling passes are required in the middle, and the total peeling amount is 0.42mm. The specific processing technology is: in the first pass, the Φ9.8mm billet is first coiled to Φ8.4mm with a processing rate of 26.5%, and then peeled to Φ8.16mm, with a peeling amount of 0.24mm; in the second pass, the Φ8.16mm billet is coiled to Φ7.4mm with a processing rate of 17.8%, and then peeled to Φ7.22mm, with a peeling amount of 0.18mm.

[0101] (4) Annealing: The Φ7.22mm wire billet is step-annealed in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 400°C in 45 minutes and kept at this temperature for 210 minutes; then, the temperature in the bell-type furnace is raised to 490°C in 20 minutes and kept at this temperature for 150 minutes; then, the temperature in the bell-type furnace is raised to 600°C in 25 minutes and kept at this temperature for 60 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 270°C. Finally, water is added for water cooling to 60°C and then the wire is taken out of the furnace at room temperature.

[0102] (5) Continuous pulling and retreating:

[0103] a. Large drawing and annealing: After bell-type furnace annealing, the Φ7.22mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ4.1mm. The processing rate is 67.8%, the stretching speed is 5mm / s, the annealing voltage is 32V, the annealing current is 1180A, and the emulsion concentration is 5.2%.

[0104] b. Continuous annealing: The Φ4.1mm wire billet is stretched to Φ1.8mm through continuous annealing, and the processing rate is controlled at 80.7%. The stretching speed is 7mm / s, the annealing voltage is 105V, the annealing current is 280A, and the emulsion concentration is 7.3%.

[0105] c. Small continuous drawing and annealing: Φ1.8mm is stretched by the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ0.6mm, with a processing rate of 88.9%.

[0106] The stretching speed was 10 mm / s, the annealing voltage was 60 V, the annealing current was 122 A, and the emulsion concentration was 8.4%.

[0107] (6) Inspect the packaging.

[0108] Example 5

[0109] A brass welding material for welding, with a specification of Φ0.6mm, is produced as follows:

[0110] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, and copper-phosphorus master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag. Then, a mixed rare earth is added and stirred sufficiently. The addition amount is 0.008wt%. Finally, the mixture is transferred into a holding furnace for insulation through a submerged liquid transfer method. The temperature is controlled at 1050-1060°C.

[0111] (2) Horizontal continuous casting: the rod billet specification is Φ9.8mm, the casting temperature is 1050-1065℃, the cooling water inlet temperature is 25℃, the water outlet temperature is 32℃, the traction pitch is 7mm, the traction time is 0.6s, the pause time is 0.10s, the reverse thrust pitch is 1.2mm, and the reverse thrust time is 0.08s.

[0112] (3) Coil pulling: The Φ9.8mm billet is first pulled in multiple passes to Φ7.22mm, with a processing rate of 45.7%. Two peeling passes are required in the middle, and the total peeling amount is 0.42mm. The specific processing technology is: in the first pass, the Φ9.8mm billet is first coiled to Φ8.4mm with a processing rate of 26.5%, and then peeled to Φ8.16mm, with a peeling amount of 0.24mm; in the second pass, the Φ8.16mm billet is coiled to Φ7.4mm with a processing rate of 17.8%, and then peeled to Φ7.22mm, with a peeling amount of 0.18mm.

[0113] (4) Annealing: The Φ7.22 mm wire billet is step-annealed in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 420°C in 45 minutes and kept at this temperature for 210 minutes; then, the temperature in the bell-type furnace is raised to 510°C in 20 minutes and kept at this temperature for 120 minutes; then, the temperature in the bell-type furnace is raised to 610°C in 25 minutes and kept at this temperature for 60 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 270°C. Finally, water is added for water cooling to 60°C and then the wire billet is taken out of the furnace at room temperature.

[0114] (5) Continuous pulling and retreating:

[0115] a. Large drawing and annealing: After bell-type furnace annealing, the Φ7.22mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ4.1mm. The processing rate is 67.8%, the stretching speed is 5mm / s, the annealing voltage is 35V, the annealing current is 1210A, and the emulsion concentration is 5.2%.

[0116] b. Continuous annealing: The Φ4.1mm wire billet is stretched to Φ1.8mm through continuous annealing, and the processing rate is controlled at 80.7%. The stretching speed is 7mm / s, the annealing voltage is 108V, the annealing current is 285A, and the emulsion concentration is 7.3%.

[0117] c. Small continuous drawing and annealing: Φ1.8mm is stretched through the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ0.6mm, with a processing rate of 88.9%.

[0118] The stretching speed was 10 mm / s, the annealing voltage was 62 V, the annealing current was 126 A, and the emulsion concentration was 8.4%.

[0119] (6) Inspect the packaging.

[0120] Example 6

[0121] A brass welding material for welding, with a specification of Φ0.6mm, is produced as follows:

[0122] (1) Smelting: electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloy, copper-iron master alloy, copper-phosphorus master alloy, and copper-indium master alloy are added into a smelting furnace according to the required proportion of alloy components and heated to melt. After the components meet the requirements, a slag remover is added to stir and remove the slag, and then mixed rare earth is added and fully stirred in an amount of 0.008wt%. Finally, the mixture is transferred into a holding furnace for insulation by a submerged liquid transfer method, and the temperature is controlled at 1050-1060°C.

[0123] (2) Horizontal continuous casting: the rod billet specification is Φ9.8mm, the casting temperature is 1050-1065℃, the cooling water inlet temperature is 25℃, the water outlet temperature is 32℃, the traction pitch is 7mm, the traction time is 0.6s, the pause time is 0.10s, the reverse thrust pitch is 1.2mm, and the reverse thrust time is 0.08s.

[0124] (3) Coil pulling: The Φ9.8mm billet is first pulled in multiple passes to Φ7.22mm, with a processing rate of 45.7%. Two peeling passes are required in the middle, and the total peeling amount is 0.42mm. The specific processing technology is: in the first pass, the Φ9.8mm billet is first coiled to Φ8.4mm with a processing rate of 26.5%, and then peeled to Φ8.16mm, with a peeling amount of 0.24mm; in the second pass, the Φ8.16mm billet is coiled to Φ7.4mm with a processing rate of 17.8%, and then peeled to Φ7.22mm, with a peeling amount of 0.18mm.

[0125] (4) Annealing: The Φ7.22 mm wire billet is step-annealed in a bell-type bright annealing furnace. The specific annealing process is as follows: first, the temperature in the bell-type furnace is raised from room temperature to 420°C in 45 minutes and kept at this temperature for 210 minutes; then, the temperature in the bell-type furnace is raised to 510°C in 20 minutes and kept at this temperature for 120 minutes; then, the temperature in the bell-type furnace is raised to 610°C in 25 minutes and kept at this temperature for 60 minutes. After the third time of keeping at this temperature, the cooling bell is replaced and air-cooled to 270°C. Finally, water is added for water cooling to 60°C and then the wire billet is taken out of the furnace at room temperature.

[0126] (5) Continuous pulling and retreating:

[0127] a. Large drawing and annealing: After bell-type furnace annealing, the Φ7.22mm wire billet is stretched by the large drawing and annealing unit and annealed online to Φ4.1mm. The processing rate is 67.8%, the stretching speed is 5mm / s, the annealing voltage is 35V, the annealing current is 1210A, and the emulsion concentration is 5.2%.

[0128] b. Continuous annealing: The Φ4.1mm wire billet is stretched to Φ1.8mm through continuous annealing, and the processing rate is controlled at 80.7%. The stretching speed is 7mm / s, the annealing voltage is 108V, the annealing current is 285A, and the emulsion concentration is 7.3%.

[0129] c. Small continuous drawing and annealing: Φ1.8mm is stretched through the small continuous drawing and annealing unit and annealed online to the finished product specification of Φ0.6mm, with a processing rate of 88.9%.

[0130] The stretching speed was 10 mm / s, the annealing voltage was 62 V, the annealing current was 126 A, and the emulsion concentration was 8.4%.

[0131] (6) Inspect the packaging.

[0132] Comparative Example 1

[0133] The HS221 tin brass welding material is produced by Hebei Jinghang Welding Materials Co., Ltd. and purchased on the market.

[0134] Comparative Example 2

[0135] The chemical composition is not consistent with the composition range of the brass welding material of the present invention, and the processing technology is consistent with that of Example 1.

[0136] Comparative Example 3

[0137] The chemical composition is consistent with that of Example 1, and the processing technology adopts the conventional process of brass welding materials, which is as follows:

[0138] A brass welding material for welding, with a specification of Φ0.6mm, is produced as follows:

[0139] (1) Smelting: Electrolytic copper, zinc ingots, tin ingots and copper-silicon master alloy are added into a smelting furnace according to the required alloy composition ratio and heated to melt. After the composition meets the requirements, a slag remover is added to stir and remove the slag. Finally, the slag is transferred into a holding furnace through a submerged liquid transfer method for insulation, and the temperature is controlled at 1050-1060℃.

[0140] (2) Horizontal continuous casting: same as Example 1.

[0141] (3) Plate pulling: the same as in Example 1.

[0142] (4) Annealing: The Φ7.22 mm wire billet is oxidatively annealed in an annealing furnace. Annealing process: annealing temperature is 540°C, heating time is 60 min, and insulation time is 240 min. After insulation is completed, the power is turned off, the furnace cover is opened, the wire billet is lifted out, and placed in the air to naturally cool to below 60°C, and then pickled to remove the oxide scale on the surface of the wire billet.

[0143] (5) Coil drawing: After pickling, the Φ7.22 mm wire billet is stretched to Φ5 mm on an inverted wire drawing machine, with a processing rate of 52%.

[0144] (6) Annealing and pickling: The Φ5mm wire billet is oxidatively annealed in the annealing furnace. The annealing process is as follows: the annealing temperature is 520°C, the heating time is 60 minutes, and the insulation time is 240 minutes. After the insulation is completed, the power is turned off, the furnace cover is opened, the wire billet is lifted out, and it is placed in the air to naturally cool to below 60°C, and then pickled to remove the oxide scale on the surface of the wire billet.

[0145] (7) Coil drawing: After pickling, the Φ5 mm wire billet is stretched to Φ3.2 mm on an inverted wire drawing machine, with a processing rate of 59%.

[0146] (8) Annealing and pickling: The Φ3.2 mm wire billet is oxidatively annealed in an annealing furnace. Annealing process: annealing temperature is 500°C, heating time is 60 min, and insulation time is 240 min. After insulation is completed, the power is turned off, the furnace cover is opened, the wire billet is lifted out, and placed in the air to naturally cool to below 60°C, and then pickled to remove the oxide scale on the surface of the wire billet.

[0147] (9) Coil drawing: After pickling, the Φ3.2 mm wire billet is stretched to Φ1.8 mm on a large water tank machine, with a processing rate of 68.3%.

[0148] (10) Annealing and pickling: The Φ1.8 mm wire billet is oxidatively annealed in an annealing furnace. Annealing process: annealing temperature is 490°C, heating time is 60 min, and insulation time is 240 min. After insulation is completed, the power is turned off, the furnace cover is opened, the wire billet is lifted out, and placed in the air to naturally cool to below 60°C, and then pickled to remove the oxide scale on the surface of the wire billet.

[0149] (11) Finished product stretching: Φ1.8mm small water tank is stretched on the machine to the finished product specification of Φ0.6mm, and the processing rate is 88.9%.

[0150] (12) Finished product annealing: The Φ1.8 mm wire billet is annealed in a hood-type bright annealing furnace. The specific annealing process is as follows: the temperature in the hood-type furnace is raised from room temperature to 400°C over 45 minutes, and then kept warm for 240 minutes. After the insulation is completed, the cooling hood is replaced and air-cooled to 270°C. Finally, water is added for water cooling to below 60°C before being taken out of the furnace.

[0151] (13)Inspect the packaging.

[0152] The thermal properties (melting point, thermal conductivity, linear expansion coefficient), corrosion resistance (maximum dezincification layer depth), microstructure (phase ratio, grain size) and welding performance of the samples prepared in the four embodiments and three comparative examples were tested, and the results are recorded in Table 2, Table 3 and Table 4, respectively.

[0153] Melting point: Heat the metal sample and measure the melting point using a differential thermal analyzer.

[0154] Thermal conductivity: measured in accordance with GB / T3651-2008 (Method for measuring high-temperature thermal conductivity of metals).

[0155] Linear expansion coefficient: measured in accordance with GB / T1039-2008 "Measurement of general temperature coefficient and general temperature shrinkage of metallic materials".

[0156] Maximum dezincification layer depth: measured in accordance with GB / T 10119-2008 "Determination of dezincification corrosion resistance of brass".

[0157] Phase ratio and grain size: The metallographic specimens were prepared in accordance with GB / T 13298. The metallographic structure was observed under a metallographic microscope. The grain size was measured according to the intercept method specified in GB / T 6394-2017 (Method for determination of average grain size of metals). The phase ratio was measured using metallographic analysis software.

[0158] Welding performance: Visual and radiographic inspections are used for welds. Visual inspections are used to observe the color, shape, and surface quality of the welds. The welds should have uniform color, a rounded shape, and a smooth surface without defects. Radiographic inspections are used to detect defects inside the welds, such as cracks, pores, slag inclusions, etc., to determine the quality of the welds.

[0159] Table 1 Chemical composition of Examples and Comparative Examples

[0160]

[0161] Table 2 Thermal performance data of embodiments and comparative examples

[0162]

[0163] Table 3 Microstructure of Examples and Comparative Examples

[0164] serial number β phase area percentage α phase size mm Example 1 1.36 0.003 Example 2 0.45 0.006 Example 3 4.68 0.009 Example 4 1.32 0.007 Example 5 0 0.007 Example 6 0 0.008 Comparative Example 1 32.22 0.035 Comparative Example 2 7.38 0.030 Comparative Example 3 1.31 0.018

[0165] Table 4 Corrosion resistance and oxidation resistance data of the embodiments and comparative examples

[0166]

[0167] like Figure 1 , Figure 2 As shown in Table 3, the brass welding materials provided by Examples 1 to 6 of the present invention have a small grain size and are evenly distributed, while the brass welding materials provided by Comparative Examples 1 to 3 have relatively coarse grains.

[0168] As shown in Table 2, the melting temperatures of the brass welding materials provided in Examples 1 to 6 of the present invention meet the range of 900-940°C, the thermal conductivity meets the range of 118-125w / (m·k), and the linear expansion coefficient meets the range of 19.2-20.4μm / (m·k); while the melting temperatures, thermal conductivity and linear expansion coefficients of Comparative Examples 1 to 3 do not meet the range required for the brass welding materials of the present invention, resulting in poor welding performance.

[0169] As shown in Table 4, the maximum dezincification layer depth of the brass welding materials provided by Examples 1 to 6 of the invention is less than 50 μm, and the brass welding materials do not change color after being baked at 250°C for 3 minutes, showing excellent corrosion resistance. Cu -(M Sn ×4+M Si ×10)≥63wt%, the maximum dezincification layer depth is only 14μm, and the corrosion resistance is better than that of Examples 1 to 4, especially Example 6, because 0.012wt% In element is added on the basis of the composition of Example 5, the maximum dezincification layer depth is only 9μm, and the corrosion resistance is the best. The maximum dezincification layer depths of Comparative Examples 1 to Comparative Examples 4 all exceed 50μm, with the maximum reaching 403μm, and oxidation discoloration occurs to varying degrees after baking at 250℃ for 3 minutes, showing poor corrosion resistance.

Claims

1. A brass welding material for welding, characterized in that: The mass percentages of the components of the brass welding material are Cu: 65-70wt%, Sn: 0.2-0.8wt%, Si: 0.05-0.6wt%, P: 0.002-0.01wt%, Fe: 0.01-0.10wt%, Pb+Bi+S≤0.01wt%, and the balance is Zn and inevitable impurities.

2. The brass welding material for welding according to claim 1, characterized in that: The contents of Cu, Sn and Si satisfy the following relationship: M Cu -(M Sn ×4+M Si ×10)≥63wt% Among them, M Cu is the content of Cu, M Si is the content of Si, M Sn is the Sn content.

3. The brass welding material for welding according to claim 1 or 2, characterized in that: The brass welding material further includes In, and the mass percentage of In is 0.003-0.018wt%.

4. The brass welding material for welding according to claim 1, characterized in that: The structure of the brass welding material for welding includes α phase and β phase, the area proportion of the β phase is less than 5%, and the size of the α phase is 0.003-0.01 mm.

5. The brass welding material for welding according to claim 1, characterized in that: The thermal properties of the brass welding material for welding are as follows: a melting point of 900-940°C, a thermal conductivity of 118-125w / (m·k), and a linear expansion coefficient of 19.2-20.4μm / (m·k) at 20-300°C.

6. A method for preparing a brass welding material for welding according to any one of claims 1 to 5, characterized in that: The process flow of the preparation method includes: smelting → horizontal continuous casting → coil drawing → annealing → continuous drawing and annealing; Wherein, the brass welding material for welding is prepared and smelted according to the mass percentage of each component as described in any one of claims 1 to 5; The continuous pulling and continuous retreating includes large pulling and continuous retreating, medium pulling and continuous retreating and small pulling and continuous retreating; The processing rate of the large-scale continuous drawing and annealing is 55-70%, the drawing speed is 2-10 mm / s, and the annealing current is 800-2000 A; The processing rate of the intermediate drawing and annealing is 65-90%, the drawing speed is 3-12 mm / s, and the annealing current is 500-800 A; The processing rate of the small continuous drawing and annealing is 60-90%, the stretching speed is 5-20 mm / s, and the annealing current is 60-300A.

7. The method for preparing a brass welding material for welding according to claim 6, characterized in that: The annealing voltage of the large continuous annealing is 20-80V, the annealing voltage of the medium continuous annealing is 30-150V, and the annealing voltage of the small continuous annealing is 50-160V.

8. The method for preparing a brass welding material for welding according to claim 6, characterized in that: Before continuous drawing and retreating, the specification of the blank is Φ5.5-8.5mm.

9. The method for preparing a brass welding material for welding according to claim 6, characterized in that: The annealing includes a gradient three-stage annealing; The annealing temperature of the first stage is 400-440°C, and the holding time is 180-240min; the annealing temperature of the second stage is 480-520°C, and the holding time is 90-210min; the annealing temperature of the third stage is 580-620°C, and the holding time is 45-90min.

10. The method for preparing brass welding material for welding according to claim 6, characterized in that: The smelting process is: mixing and melting the raw materials according to the mass percentage of each component of the brass welding material for welding according to any one of claims 1 to 5, then adding a slag cleaning agent to stir and remove the slag, and then adding a mixed rare earth element, wherein the mixed rare earth element mainly consists of Ce, La, Nd and Pr; The raw materials include electrolytic copper, zinc ingots, tin ingots, copper-silicon master alloys, copper-iron master alloys, copper-phosphorus master alloys or copper-indium master alloys, and the order of adding materials is electrolytic copper→copper-silicon master alloys and copper-iron master alloys→zinc ingots→tin ingots→copper-indium master alloys→copper-phosphorus master alloys.

11. The method for preparing a brass welding material for welding according to claim 6, characterized in that: The temperature of the horizontal continuous casting is 1040-1070° C., the pulling pitch is 4-15 mm, the pulling time is 0.05-0.6 s, the pulling stop time is 0.01-0.2 s, the reverse thrust pitch is 0.4-3 mm, and the reverse thrust time is 0.02-0.3 s.

12. The method for preparing a brass welding material for welding according to claim 6, characterized in that: The process of coiling is: first stretching→first peeling→second stretching→second peeling; Among them, the processing rate of the first extension is 20-30%, the peeling amount of the first peeling is 0.2-0.3mm, the processing rate of the second extension is 10-25%, and the peeling amount of the second peeling is 0.15-0.25mm.

Citation Information

Patent Citations

  • Tin brass alloy welding flux

    CN109434318A

  • Easily-welded brass and preparation method thereof

    CN115354188A