Anti-cracking silicon core pipe and preparation method thereof

By using composite structure and specific additives in the silicon core tube, the problem of silicon core tube prone to cracking in the underground environment is solved, and its crack resistance and stability is significantly improved, meeting the needs of impact resistance and heat resistance.

CN119078295APending Publication Date: 2024-12-06HEBEI KUNPENG PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411212389.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional silicon core tubes are prone to cracks in underground environments, resulting in pipeline failure or leakage, and lack good crack resistance.

Method used

Adopt the composite structure of the outer layer and the inner layer. The outer layer consists of high-density polyethylene, ethylene-octene copolymer, filler and flame retardant. The inner layer is composed of polydimethylsiloxane, ethylene-octene copolymer and resistor. The combustion agent is composed of a fueling agent, and 4,4'-dihydroxydiphenyl sulfide and p-aminophenol are added to the additive, and the silicon core tube is prepared by a synchronous extrusion composite process.

Benefits of technology

It improves the crack resistance of silicon core tubes, enhances its impact, heat and oxidation resistance, delays the material aging process, and significantly improves the stability and crack resistance of the pipeline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of silicon core pipes, and provides an anti-cracking silicon core pipe and a preparation method thereof. The anti-cracking silicon core pipe comprises an outer layer and an inner layer, and the outer layer is prepared from, by weight, 70-90 parts of high-density polyethylene, 10-15 parts of ethylene-octylene copolymer, 10-15 parts of filler, 1-3 parts of flame retardant and 6-10 parts of auxiliaries; the inner layer is prepared from the following raw materials in parts by weight: 8 to 10 parts of polydimethylsiloxane, 70 to 90 parts of high-density polyethylene, 10 to 15 parts of ethylene-octylene copolymer and 1 to 3 parts of flame retardant; the auxiliary agent comprises 4, 4 '-dihydroxy diphenyl sulfide and / or p-aminophenol. By means of the technical scheme, the problem that in the prior art, the anti-cracking performance of the silicon core pipe is low is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon core tubes, and in particular to an anti-cracking silicon core tube and a preparation method thereof. Background Art

[0002] With the development of the electric power industry, the demand for protection of power cables is getting higher and higher. Traditional cable protection materials such as metal pipes have problems such as heavy weight, corrosion, and poor insulation performance. In order to solve these problems, scientists and engineers began to study new cable protection materials, including HDPE silicon core pipes. HDPE silicon core pipe is a pipe product composed of high-density polyethylene (HDPE) and silicon core, which is usually used in underground communications, power cables and other fields. When silicon core pipes are used in underground communications, due to the complexity and variability of the underground environment, the pipeline may be subjected to various stresses and loads, such as earthquakes, ground deformation, mechanical extrusion, etc. If the silicon core pipe does not have good crack resistance, it is easy to crack under external stress, resulting in pipeline failure or leakage. Therefore, the development of a crack-resistant silicon core pipe is an urgent problem to be solved. Summary of the invention

[0003] The invention provides an anti-cracking silicon core tube and a preparation method thereof, which solves the problem of low anti-cracking performance of the silicon core tube in the related art.

[0004] The technical solution of the present invention is as follows: The present invention provides an anti-cracking silicon core tube, comprising an outer layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 70-90 parts of high-density polyethylene, 10-15 parts of ethylene-octene copolymer, 10-15 parts of filler, 1-3 parts of flame retardant, and 6-10 parts of auxiliary agent; The inner layer comprises the following raw materials in parts by weight: 8-10 parts of polydimethylsiloxane, 70-90 parts of high-density polyethylene, 10-15 parts of ethylene-octene copolymer, and 1-3 parts of flame retardant; The auxiliary agent includes 4,4'-dihydroxydiphenyl sulfide and / or p-aminophenol.

[0005] As a further technical solution, the ethylene-octene copolymer consists of a first ethylene-octene copolymer and a second ethylene-octene copolymer, and the first ethylene-octene copolymer and the second ethylene-octene copolymer have different melt flow rates.

[0006] As a further technical solution, the mass ratio of the first ethylene-octene copolymer to the second ethylene-octene copolymer is 1-3:1.

[0007] As a further technical solution, the mass ratio of the first ethylene-octene copolymer to the second ethylene-octene copolymer is 2:1.

[0008] As a further technical solution, the melt flow rate of the first ethylene-octene copolymer is 3 g / 10 min, and the melt flow rate of the second ethylene-octene copolymer is 12 g / 10 min.

[0009] As a further technical solution, when the auxiliary agent is composed of 4,4'-dihydroxydiphenyl sulfide and p-aminophenol, the mass ratio of the 4,4'-dihydroxydiphenyl sulfide to p-aminophenol is 2-4:1.

[0010] As a further technical solution, the mass ratio of the 4,4'-dihydroxydiphenyl sulfide to p-aminophenol is 3:1.

[0011] As a further technical solution, the filler includes one or both of carbon black and carbon nanotubes.

[0012] As a further technical solution, the flame retardant includes one or two of sodium hexametaphosphate and hexabromobiphenyl.

[0013] The present invention also provides a method for preparing a crack-resistant silicon core tube, comprising the following steps: S1, mixing the outer layer raw materials uniformly to obtain an outer layer mixture; S2, mixing the inner layer raw materials uniformly to obtain an inner layer mixture; S3, after the outer layer mixture and the inner layer mixture are heated and melted respectively, they are extruded and compounded simultaneously, and after shaping, a silicon core tube is obtained.

[0014] As a further technical solution, the outer layer raw material mixing temperature is 140-160° C., and the mixing time is 50-70 min.

[0015] As a further technical solution, the inner layer raw materials are mixed at a temperature of 120-130° C. and a mixing time of 30-40 min.

[0016] The working principle and beneficial effects of the present invention are: In the present invention, an ethylene-octene copolymer is added, and the molecular weight distribution of the copolymer is relatively narrow. The side octyl group in the molecular structure is longer than the side ethyl group, and a connection point can be formed in the molecular structure, which plays a role of connection and buffering between the components, so that when the system is impacted, the chance of silver streaks developing into cracks due to stress is reduced, and the silicon core tube has a good anti-cracking effect; 4,4'-dihydroxydiphenyl sulfide and / or p-aminophenol are added as auxiliary agents to the outer layer of the silicon core tube, which can effectively improve the antioxidant capacity and heat resistance of the silicon core tube, and further improve the anti-cracking performance of the silicon core tube. Among them, the sulfide group of 4,4'-dihydroxydiphenyl sulfide can improve the heat resistance of HDPE pipes, reduce thermal oxidation decomposition and degradation reactions, thereby improving the anti-cracking performance; the phenylamino group in p-aminophenol captures free radicals and active oxidizing substances, prevents the oxidation chain reaction of polymer materials, inhibits the oxidative degradation process of polymers, delays the aging of materials, enhances the stability of pipes, and thus improves the anti-cracking performance of silicon core tubes. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] In the following embodiments and comparative examples: High-density polyethylene: model number is P4406C, the manufacturer is Suzhou Jedamin Plastic Raw Materials Co., Ltd.; The first ethylene-octene copolymer has a melt flow rate of 3g / 10min and is manufactured by Dongguan Hongchuang Plastic Co., Ltd. The second ethylene-octene copolymer has a melt flow rate of 12 g / 10 min and is manufactured by Dongguan Hongchuang Plastic Co., Ltd. Polydimethylsiloxane: model is ST-30, content is 30%, manufacturer is Suzhou Jingyu Biotechnology Co., Ltd.

[0019] Example 1 S1, weigh 70 parts of high-density polyethylene, 10 parts of the first ethylene-octene copolymer, 10 parts of carbon black, 1 part of sodium hexametaphosphate, and 6 parts of 4,4'-dihydroxydiphenyl sulfide, heat to 140°C, stir for 70 minutes, mix evenly, and obtain an outer layer mixture; S2, weigh 8 parts of polydimethylsiloxane, 70 parts of high-density polyethylene, 10 parts of the first ethylene-octene copolymer, and 1 part of sodium hexametaphosphate, raise the temperature to 120° C., stir for 40 minutes, mix evenly, and obtain an inner layer mixture; S3, after the outer layer mixture and the inner layer mixture are heated and melted respectively, they are extruded and compounded simultaneously, and after shaping, a silicon core tube is obtained.

[0020] Example 2 S1, weigh 80 parts of high-density polyethylene, 12 parts of the first ethylene-octene copolymer, 12 parts of carbon black, 2 parts of sodium hexametaphosphate, and 8.4 parts of 4,4'-dihydroxydiphenyl sulfide, heat to 150°C, stir for 60 minutes, mix evenly, and obtain an outer layer mixture; S2, weigh 9 parts of polydimethylsiloxane, 80 parts of high-density polyethylene, 12 parts of the first ethylene-octene copolymer, and 2 parts of sodium hexametaphosphate, raise the temperature to 125° C., stir for 35 minutes, mix evenly, and obtain an inner layer mixture; S3, after the outer layer mixture and the inner layer mixture are heated and melted respectively, they are extruded and compounded simultaneously, and after shaping, a silicon core tube is obtained.

[0021] Example 3 S1, weigh 90 parts of high-density polyethylene, 15 parts of the first ethylene-octene copolymer, 15 parts of carbon nanotubes, 3 parts of hexabromobiphenyl, and 10 parts of 4,4'-dihydroxydiphenyl sulfide, heat to 160°C, stir for 50 minutes, mix evenly, and obtain an outer layer mixture; S2, weigh 10 parts of polydimethylsiloxane, 90 parts of high-density polyethylene, 15 parts of the first ethylene-octene copolymer, and 3 parts of hexabromobiphenyl, heat to 130° C., stir for 30 minutes, mix evenly, and obtain an inner layer mixture; S3, after the outer layer mixture and the inner layer mixture are heated and melted respectively, they are extruded and compounded simultaneously, and after shaping, a silicon core tube is obtained.

[0022] Example 4 Compared with Example 2, Example 4 is different in that the first ethylene-octene copolymer is replaced by an equal amount of the second ethylene-octene copolymer.

[0023] Example 5 Compared with Example 2, Example 5 is different in that 12 parts of the first ethylene-octene copolymer is replaced by 9.6 parts of the first ethylene-octene copolymer and 2.4 parts of the second ethylene-octene copolymer.

[0024] Example 6 Compared with Example 2, Example 6 is different in that 12 parts of the first ethylene-octene copolymer is replaced by 9 parts of the first ethylene-octene copolymer and 3 parts of the second ethylene-octene copolymer.

[0025] Example 7 Compared with Example 2, Example 7 is different in that 12 parts of the first ethylene-octene copolymer is replaced by 8 parts of the first ethylene-octene copolymer and 4 parts of the second ethylene-octene copolymer.

[0026] Example 8 Compared with Example 2, Example 8 is different in that 12 parts of the first ethylene-octene copolymer is replaced by 6 parts of the first ethylene-octene copolymer and 6 parts of the second ethylene-octene copolymer.

[0027] Example 9 Compared with Example 2, Example 9 is different in that 12 parts of the first ethylene-octene copolymer is replaced by 4 parts of the first ethylene-octene copolymer and 8 parts of the second ethylene-octene copolymer.

[0028] Example 10 Compared with Example 7, Example 10 is different in that 4,4'-dihydroxydiphenyl sulfide is replaced by an equal amount of p-aminophenol.

[0029] Embodiment 11 Compared with Example 7, Example 11 is different in that 8.4 parts of 4,4'-dihydroxydiphenyl sulfide are replaced by 4.2 parts of 4,4'-dihydroxydiphenyl sulfide and 4.2 parts of p-aminophenol.

[0030] Example 12 Compared with Example 7, Example 12 is different in that 8.4 parts of 4,4'-dihydroxydiphenyl sulfide are replaced with 5.6 parts of 4,4'-dihydroxydiphenyl sulfide and 2.8 parts of p-aminophenol.

[0031] Example 13 Compared with Example 7, Example 13 is different in that 8.4 parts of 4,4'-dihydroxydiphenyl sulfide are replaced with 6.3 parts of 4,4'-dihydroxydiphenyl sulfide and 2.1 parts of p-aminophenol.

[0032] Embodiment 14 Compared with Example 7, Example 14 is different in that 8.4 parts of 4,4'-dihydroxydiphenyl sulfide is replaced by 6.72 parts of 4,4'-dihydroxydiphenyl sulfide and 1.68 parts of p-aminophenol.

[0033] Embodiment 15 Compared with Example 7, Example 15 is different in that 8.4 parts of 4,4'-dihydroxydiphenyl sulfide are replaced by 7 parts of 4,4'-dihydroxydiphenyl sulfide and 1.4 parts of p-aminophenol.

[0034] Example 16 Compared with Example 2, Example 16 is different in that the first ethylene-octene copolymer is replaced with an equal amount of ethylene-octene copolymer, and the melt flow rate is 1 g / 10 min.

[0035] Embodiment 17 Compared with Example 2, Example 17 is different in that the first ethylene-octene copolymer is replaced with an equal amount of ethylene-octene copolymer, and the melt flow rate is 30 g / 10 min.

[0036] Comparative Example 1 Compared with Example 2, Comparative Example 1 is different in that 4,4′-dihydroxydiphenyl sulfide is not added.

[0037] The crack-resistant silicon core tubes prepared in Examples 1 to 17 and Comparative Example 1 were tested according to the following method: 1. Elongation at break: According to the test method specified in GB / T 24456-2009 "High-density polyethylene silicon core tube", the elongation at break of the test sample is tested.

[0038] 2. Resistance to environmental stress cracking: Test the environmental stress cracking resistance of the samples according to the test method specified in GB / T 24456-2009 "High-density polyethylene silicon core tube".

[0039] The test results are shown in the following table: Table 1 Performance test results of silicon core tubes prepared in Examples 1 to 17 and Comparative Example 1

[0040] Compared with Example 2 and Example 4, the melt flow rate of the ethylene-octene copolymer added in Example 16 is 1 g / 10 min, and the melt flow rate of the ethylene-octene copolymer added in Example 17 is 30 g / 10 min. As a result, the elongation at break and the environmental crack resistance time of Example 2 and Example 4 are higher than those of Example 16 and Example 17, indicating that when the melt flow rate of the ethylene-octene copolymer is in the range of 3~12 g / 10 min, the elongation at break of the silicon core tube is the largest and the anti-cracking performance is better.

[0041] Compared with Example 2 and Example 4, Examples 5 to 9 simultaneously added the first ethylene-octene copolymer and the second ethylene-octene copolymer. As a result, the elongation at break and the environmental cracking resistance time of Examples 5 to 9 were higher than those of Examples 2 and Example 4, indicating that the first ethylene-octene copolymer and the second ethylene-octene copolymer play a synergistic role and can further enhance the elongation at break and the cracking resistance of the silicon core tube.

[0042] Compared with Example 5, Examples 6 to 9 added different proportions of the first ethylene-octene copolymer and the second ethylene-octene copolymer. As a result, the elongation at break and the environmental cracking resistance time of Examples 6 to 8 were higher than those of Examples 5 and 9, indicating that when the mass ratio of the first ethylene-octene copolymer to the second ethylene-octene copolymer is 1 to 3:1, and the preferred ratio is 2:1, the elongation at break of the silicon core tube is the largest and the anti-cracking performance is better.

[0043] Compared with Comparative Example 1, Example 2 adds 4,4'-dihydroxydiphenyl sulfide. As a result, the elongation at break and the environmental cracking resistance time of Example 2 are higher than those of Comparative Example 1, indicating that the addition of 4,4'-dihydroxydiphenyl sulfide can enhance the elongation at break and the cracking resistance of the silicon core tube.

[0044] Compared with Example 10, Examples 11 to 15 simultaneously added 4,4'-dihydroxydiphenyl sulfide and p-aminophenol. As a result, the elongation at break and the environmental cracking resistance time of Examples 11 to 15 were higher than those of Example 10, indicating that 4,4'-dihydroxydiphenyl sulfide and p-aminophenol played a synergistic role and could further enhance the elongation at break and the cracking resistance of the silicon core tube.

[0045] Compared with Example 11, Examples 12 to 15 added different proportions of 4,4'-dihydroxydiphenyl sulfide and p-aminophenol. As a result, the elongation at break and the environmental cracking resistance time of Examples 12 to 14 were higher than those of Examples 11 and 15, indicating that when the mass ratio of 4,4'-dihydroxydiphenyl sulfide and p-aminophenol was 2 to 4:1, and the preferred ratio was 3:1, the elongation at break of the silicon core tube was the largest and the anti-cracking performance was the best.

[0046] Referring to the test method specified in the standard GB / T 24456-2009 "High-density polyethylene silicon core tube", the appearance, drop hammer impact resistance, cold bending radius, chemical medium corrosion resistance, hydraulic resistance, thermal stress cracking resistance, and inner wall friction coefficient of Examples 1 to 17 were tested, and the test results are as follows: Appearance: The color is uniform, the inner and outer surfaces are flat, uniform and smooth, without defects such as collapse, pits, holes, tear marks and impurity pits, the cross-section is bright, without bubbles or cracks, the inner wall of the silicon core tube is tightly sintered without detachment, all meeting the requirements.

[0047] Drop hammer impact resistance: At the specified temperature (normal temperature 23℃, low temperature -20℃), at a height of 2m, a 15.3kg hammer impacted 10 specimens, and none of the 10 specimens showed cracking, meeting the qualification standards.

[0048] Cold bending radius: No cracking, cracking or obvious stress whitening.

[0049] Resistance to chemical corrosion: The samples were immersed in 5% NaCl, 40% H2SO4 and 40% NaOH solutions for 24 hours respectively, and there was no obvious fading or corrosion.

[0050] Hydraulic resistance: Under the conditions of temperature 20℃ and water pressure 2.0MPa, maintained for 15min, there are no visible cracks on the samples.

[0051] Resistance to thermal stress cracking: 168h, failure rate is 0.

[0052] Inner wall friction coefficient: static ≤0.25, all samples passed.

[0053] Therefore, the silicon core tubes of Examples 1 to 17 of the present invention all meet the relevant requirements of the standard GB / T 24456-2009 "High-density polyethylene silicon core tube".

[0054] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A crack-resistant silicon core tube, It is characterized in that It comprises an outer layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 70-90 parts of high-density polyethylene, 10-15 parts of ethylene-octene copolymer, 10-15 parts of filler, 1-3 parts of flame retardant, and 6-10 parts of additive; The inner layer comprises the following raw materials in parts by weight: 8-10 parts of polydimethylsiloxane, 70-90 parts of high-density polyethylene, 10-15 parts of ethylene-octene copolymer, and 1-3 parts of flame retardant; the auxiliary agent comprises 4,4'-dihydroxydiphenyl sulfide and / or p-aminophenol.

2. The anti-cracking silicon core tube according to claim 1, It is characterized in that The ethylene-octene copolymer consists of a first ethylene-octene copolymer and a second ethylene-octene copolymer, and the first ethylene-octene copolymer and the second ethylene-octene copolymer have different melt flow rates.

3. The anti-cracking silicon core tube according to claim 2, It is characterized in that The mass ratio of the first ethylene-octene copolymer to the second ethylene-octene copolymer is 1-3:

1.

4. The anti-cracking silicon core tube according to claim 1, It is characterized in that The melt flow rate of the ethylene-octene copolymer is 3-12 g / 10 min.

5. The anti-cracking silicon core tube according to claim 1, It is characterized in that When the auxiliary agent consists of 4,4'-dihydroxydiphenyl sulfide and p-aminophenol, the mass ratio of the 4,4'-dihydroxydiphenyl sulfide to p-aminophenol is 2-4:

1.

6. The anti-cracking silicon core tube according to claim 1, It is characterized in that The filler includes one or both of carbon black and carbon nanotubes.

7. The anti-cracking silicon core tube according to claim 1, It is characterized in that The flame retardant includes one or two of sodium hexametaphosphate and hexabromobiphenyl.

8. A method for preparing a crack-resistant silicon core tube according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1, mixing the outer layer raw materials uniformly to obtain an outer layer mixture; S2, mixing the inner layer raw materials uniformly to obtain an inner layer mixture; S3, after the outer layer mixture and the inner layer mixture are heated and melted respectively, they are extruded and compounded simultaneously, and after shaping, a silicon core tube is obtained.

9. A method for preparing a crack-resistant silicon core tube according to claim 8, It is characterized in that The outer layer raw materials are mixed at a temperature of 140-160° C. and a mixing time of 50-70 min.

10. The method for preparing a crack-resistant silicon core tube according to claim 1, It is characterized in that The inner layer raw materials are mixed at a temperature of 120-130° C. and a mixing time of 30-40 minutes.