Comprehensive treatment method and device for iron element in iron-containing alloy
The controlled chlorination and oxidation process for iron-containing alloys simplifies and reduces costs by preferentially separating iron, producing high-quality iron oxide while recycling chlorine, addressing the inefficiencies of traditional metallurgical methods.
Patent Information
- Application Number
- CN202411206334.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
Existing methods for processing iron-containing alloys are lengthy, environmentally burdensome, and energy-intensive due to the use of metallurgical processes that do not selectively separate iron and nickel, leading to complex impurity removal and high energy consumption.
A comprehensive treatment method involving roasting in a chlorine atmosphere to produce ferrous chloride melt, followed by chlorination to convert it into ferric chloride gas, and subsequent oxidation with oxygen to obtain iron oxide, utilizing a controlled chlorination process to preferentially separate iron.
This method achieves a short process flow with high-quality iron oxide production, reduces production costs by recycling chlorine, and enhances operational simplicity.
Smart Images

Figure CN119080070A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ferrous alloy processing, and in particular to a comprehensive processing method and device for iron elements in ferrous alloys. Background Art
[0002] The efficient and fine separation of valuable elements in alloys and even waste alloys, such as copper-cobalt alloys and waste high-temperature alloys, has always been a difficult point in research. At present, the methods for resource utilization of waste alloys that have been studied include mechanical crushing, zinc melting, oxidation-reduction, electrochemical, and biological leaching. However, due to the stubborn properties of alloys, such as high hardness, density, corrosion resistance, and wear resistance, and the fact that most elements exist in the form of intermetallic compounds, most processes use metallurgical methods with "three highs and one strong", which leads to problems such as long process flow, heavy environmental load, and high energy consumption. It is urgent to develop short-process, high-efficiency, high-quality, and low-cost waste alloy processing technology.
[0003] The above-mentioned method for high-value utilization of iron-containing alloys mainly involves first using reagents to wet-leach the iron-containing alloy to destroy the dense structure of the iron-containing alloy, while allowing nickel, iron, etc. in the alloy to enter the solution, and then the solution is purified and partially extracted for valuable metals. When the above-mentioned method is used to leach the iron-containing alloy, both nickel and iron enter the leachate, which is not selective, resulting in subsequent lengthy extraction processes such as impurity removal and separation. Summary of the invention
[0004] The main purpose of the present invention is to provide a comprehensive treatment method and device for iron in iron-containing alloys to solve the technical problem of lengthy iron separation procedures.
[0005] To achieve the above object, the present invention provides a comprehensive treatment method for iron in an iron-containing alloy, comprising the following steps:
[0006] The iron-containing alloy is roasted in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and the ferrous chloride melt is separated, wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the iron-containing alloy, and the roasting temperature is 500 to 850°C.
[0007] Chlorine gas is introduced into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas, wherein the temperature of the chlorination reaction is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt.
[0008] The ferric chloride gas is drawn out to react with oxygen to obtain iron oxide and recover chlorine, wherein the reaction temperature is 700-1200° C. and the amount of oxygen introduced is 0.75-1.1 times the volume of the ferric chloride gas.
[0009] According to the implementation mode of the present application, it also includes:
[0010] The recovered chlorine gas is introduced into the iron-containing alloy to form the chlorine gas atmosphere.
[0011] The present application also provides a comprehensive treatment device for iron in ferroalloys, comprising:
[0012] The roasting furnace comprises a furnace body and a first chlorine gas inlet, wherein the furnace body has a containing cavity for containing the iron-containing alloy, the first chlorine gas inlet is connected to the containing cavity, and the mass of the introduced chlorine gas is 0.8 to 1.5 times the mass of the iron-containing alloy. The roasting temperature in the furnace body is 500 to 850°C.
[0013] A separation mechanism is communicated with the accommodating cavity and is used to separate the ferrous chloride melt generated by the furnace body.
[0014] The chlorination reaction chamber has a second chlorine gas inlet, the chlorination reaction chamber is connected with the separation mechanism, and the chlorination reaction chamber receives the ferrous chloride melt and reacts it with the second chlorine gas to generate ferric chloride gas.
[0015] The oxidation reaction chamber has an oxygen inlet and a chlorine outlet. The oxidation reaction chamber is connected to the chlorination reaction chamber, and the oxidation reaction chamber receives the ferric chloride gas and reacts it with oxygen to obtain ferric oxide and recover chlorine.
[0016] The iron oxide collection chamber is connected to the oxidation reaction chamber to collect and recycle the iron oxide.
[0017] According to an embodiment of the present application, the separation mechanism includes a plurality of connecting pipes evenly distributed on the bottom surface of the furnace body, forming a pipeline for separating the ferrous chloride melt. The plurality of connecting pipes each include a first end and a second end opposite to each other. The first end extends into the furnace body and exceeds the bottom of the furnace body, and the second end is connected to the chlorination reaction chamber.
[0018] The opening of the first chlorine gas inlet close to the furnace body is located in the area between the first end and the bottom of the furnace body. The first chlorine gas inlet and the connecting pipe are alternately distributed.
[0019] According to an embodiment of the present application, the first chlorine gas inlet is arranged to be inclined downward from outside the furnace body to inside the furnace body, and a shielding portion for preventing the iron-containing alloy from entering the connecting pipe is provided at the end of the first end of the connecting pipe.
[0020] According to an embodiment of the present application, the connecting pipe includes a bending section that bends back and forth along the height direction of the furnace body.
[0021] Portions of the plurality of connecting pipes within the furnace body are retractable.
[0022] According to the embodiment of the present application, it also includes a top sealing device and a feeding mechanism.
[0023] The top sealing device is located at the top of the furnace body and is used for sealing the furnace body.
[0024] The feeding mechanism comprises:
[0025] The alloy introduction port comprises a plurality of introduction channels which are connected with the furnace body through the top sealing device.
[0026] The pre-installed component is funnel-shaped, and its bottom is connected with the alloy inlet away from the furnace body. The bottom of the pre-installed component is provided with a first sealed switch.
[0027] The alloy adding port is communicated with the top of the preassembled component, and the alloy adding port is provided with a second sealed switch.
[0028] According to an embodiment of the present application, the second chlorine gas inlet includes a side inlet and a bottom inlet.
[0029] The side air inlets are located at the lower part of the side of the chlorination reaction chamber away from the oxidation reaction chamber, and are evenly distributed vertically.
[0030] The bottom air inlet is located at the bottom of the chlorination reaction chamber and is evenly distributed in an area extending 2 / 3 along the length direction from one side of the oxidation reaction chamber.
[0031] The comprehensive treatment device also includes a one-way air intake mechanism that connects the chlorination reaction chamber to the oxidation reaction chamber.
[0032] According to an embodiment of the present application, the oxygen inlet extends from the side into the interior of the oxidation reaction chamber and is located at a height of 1 / 2-2 / 3 from the top of the chamber.
[0033] According to an embodiment of the present application, the oxidation reaction chamber further includes an online monitoring device for chlorine and oxygen content and a ferric chloride gas addition port.
[0034] In the above-mentioned comprehensive treatment method of iron in the iron-containing alloy, by controlling the chlorination conditions, the preferential chlorination of iron in the alloy is achieved, and it is converted into molten ferrous chloride. Then the ferrous chloride is converted into gaseous ferric chloride and volatilized, and cooled to obtain ferric chloride. The ferric chloride is reoxidized to obtain iron oxide and recycle chlorine. The element behavior of iron in the alloy is to convert from solid alloy to liquid ferrous chloride, then to gaseous ferric chloride, and finally to iron oxide, which realizes the continuity of the process. And in the process of molten ferrous chloride gasification, the reaction can be well controlled, and high-quality ferric chloride can be prepared. The recovered chlorine can be used directly or as chlorine after purification, thereby reducing production costs. The above-mentioned comprehensive treatment method of iron in the iron-containing alloy is simple to operate, has a short process flow, and obtains high-quality iron oxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0036] Figure 1 It is a schematic structural diagram of a comprehensive treatment device for iron elements in an iron-containing alloy according to an embodiment of the present application;
[0037] Figure 2 is a top view of the bottom structure of a roasting furnace according to an embodiment of the present application;
[0038] Figure 3 is a top view of a chlorination reaction chamber of a roasting furnace according to an embodiment of the present application;
[0039] Figure 4 It is a top view of the internal structure of the iron oxide collection chamber of the roasting furnace according to one embodiment of the present application;
[0040] Figure 5 It is a ferrous chloride melt sample according to an embodiment of the present application;
[0041] Figure 6 It is a ferric chloride sample according to one embodiment of the present application;
[0042] Figure 7 is a SEM image of a ferric chloride sample according to an embodiment of the present application;
[0043] Figure 8 It is an XRD diagram of a ferric chloride sample according to one embodiment of the present application.
[0044] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings.
[0045] 100, roasting furnace; 200, separation mechanism; 300, chlorination reaction chamber; 400, oxidation reaction chamber; 500, top sealing device; 600, feeding mechanism; 700, iron oxide collection chamber;
[0046] 210, connecting pipe; 211, shielding portion; 212, bending section;
[0047] 610, alloy insertion port; 620, pre-installed components; 630, alloy addition port; 611, insertion channel; 621, first sealed switch; 631, second sealed switch;
[0048] 110. first chlorine gas inlet; 120. furnace body; 130. temperature control and heat preservation device;
[0049] 310, second chlorine gas inlet; 311, side air inlet; 312, bottom air inlet; 320, first temperature control device; 330, one-way air inlet mechanism;
[0050] 410, chlorine and oxygen content online monitoring device; 420, ferric chloride gas supply port; 430, chlorine gas discharge port; 440, second temperature control device; 450, oxygen inlet;
[0051] 710, first discharging chamber; 720, second discharging chamber; 730, third sealed switch; 740, fourth sealed switch. DETAILED DESCRIPTION
[0052] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0054] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0055] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0056] The present invention provides a comprehensive treatment method for iron in an iron-containing alloy, comprising the following steps:
[0057] S100: roasting the iron-containing alloy in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and separating the ferrous chloride melt, wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the iron-containing alloy, and the roasting temperature is 500 to 850°C.
[0058] The present invention provides a comprehensive treatment method for iron in an iron-containing alloy, and the overall idea is as follows: by controlling the chlorination conditions, the iron in the alloy is preferentially chlorinated and converted into molten ferrous chloride. The unreacted iron-containing alloy and the solid slag obtained by the reaction are both solid, and the molten ferrous chloride is liquid, which is easy to separate from the solid, such as by filtering, centrifugation, etc. Specifically in some embodiments, a filter hole is set at the bottom of the reaction container (such as a roasting furnace) of the iron-containing alloy, so that the molten ferrous chloride is filtered out from the bottom of the container.
[0059] In the subsequent step, chlorine gas is introduced into the obtained molten ferrous chloride to convert the ferrous chloride into gaseous ferric chloride and volatilize it.
[0060] Oxygen is introduced into the volatilized gaseous ferric chloride to react and produce iron oxide and chlorine. In order to distinguish it from the chlorine introduced into the iron-containing alloy, the chlorine produced in this step is called recovered chlorine.
[0061] The iron-containing alloy of the embodiment of the present application includes nickel-iron alloy. Taking nickel-iron alloy as an example, it is an alloy whose main components are nickel and iron, and is a smelting intermediate. In some embodiments, the iron-containing alloy of the embodiment of the present application is an iron-containing alloy obtained by pyrometallurgical smelting of laterite nickel ore, such as RK-EF method, rotary kiln direct reduction-magnetic separation process, rotary hearth furnace-melting furnace process. In some specific embodiments, the composition of the iron-containing alloy is shown in Table 1.
[0062] Table 1: Chemical composition of iron-containing alloys (wt%)
[0063]
[0064] In step S100, the mass ratio of chlorine to the mass of the iron-containing alloy and the roasting temperature are controlled to achieve preferential chlorination of the iron in the alloy. When the roasting temperature and the chlorine content are too high, both nickel and iron generate chlorides, nickel generates gaseous nickel chloride, and iron generates gaseous ferrous chloride or gaseous ferric chloride, thereby failing to achieve the effect of solid-liquid separation. When the roasting temperature and the chlorine content are too low, iron generates less or no ferric chloride, and similarly failing to achieve the effect of solid-liquid separation.
[0065] The specific roasting time is not specifically required, and the ferrous chloride melt is produced. In particular, in some embodiments, a continuous comprehensive treatment method of iron from the ferrous alloy is adopted. The total amount of the ferrous alloy is large, and step S100 is a process of continuous reaction, in which the ferrous alloy is added in a large amount at one time or continuously added to the ferrous alloy, and in the roasting process, ferrous chloride melt and solid slag are continuously generated. As the reaction proceeds, the solid slag after the reaction is completed can also be separated.
[0066] In some specific embodiments, the mass of the chlorine gas is 0.8 to 1.5 times the mass of the iron-containing alloy, and the calcination temperature is 600 to 800°C.
[0067] In step S100, possible reaction equations include:
[0068] Ni-Fe+Cl 2 (g) →FeCl 2 (l)+NiCl 2 (s)+Ni(s),FeCl 2 (l)+Cl 2 (g)
[0069] →FeCl 3 (g), FeCl 3 (g)+Fe(s)→FeCl 2 (l);FeCl 3 (g) → Cl 2 (g)+FeCl 2 (g).
[0070] First, the present invention controls the reaction conditions and the amount of chlorine added is small, so FeCl 2 (l) Continue to react to generate FeCl 3 (g) Not easy to carry out.
[0071] Secondly, due to the small amount of chlorine added, the iron in the iron-containing alloy is relatively excessive, and the excess iron reacts with FeCl 3 (g) Continue to react to form FeCl 2 (l) FeCl 2(l) Continuously separate from the reaction system to promote the reaction to continue to generate FeCl 2 (l) is carried out, consuming FeCl 3 (g).
[0072] Again, studies have shown that (Performance evaluation of the Fe–Cl and Mg–Cl cycle for hydrogen production of the minor actinide fuelled PACER fusion blanket) FeCl 3 At high temperature (698K, 424.85℃), it will decompose to form FeCl 2 +Cl 2 , thus further promoting the formation of ferrous chloride at some reaction temperatures of the present application, and consuming FeCl 3 (g).
[0073] Therefore, under the influence of the above factors, the main product in step S100 of the present application is FeCl 2 (l) That is, molten ferric chloride, not ferric chloride.
[0074] In some more specific embodiments, the mass of the chlorine gas is 0.9 to 1.2 times the mass of the iron-containing alloy, and the calcination temperature is 650 to 750°C.
[0075] S200: introducing chlorine gas into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas; wherein the temperature of the chlorination reaction is 400-700° C., and the amount of chlorine gas introduced is 0.25-0.35 times the mass of the ferrous chloride melt.
[0076] In the process of molten ferrous chloride being gasified by chlorine, the reaction can be well controlled, and high-quality ferric chloride can be prepared. For example, ferrous chloride melt is placed in a chlorination reaction chamber, and chlorine is introduced into the molten ferrous chloride to cause a chlorination reaction between the two.
[0077] For example, if an iron-containing alloy is treated in one step to convert iron into ferric chloride, it is difficult to continue the one-step treatment. For example, when there is only a small amount of alloy in the later stage of the reaction, it is difficult for the introduced chlorine to contact the alloy, resulting in low utilization rate of chlorine.
[0078] After adopting the step-by-step treatment, one furnace is specifically responsible for the production of ferrous chloride, that is, when one batch of alloy has not yet completely reacted, the second batch of materials is added, and then the third batch of materials. The addition of materials can not only ensure the formation of ferrous chloride, but also ensure the contact efficiency between chlorine and alloy due to the high material content.
[0079] Moreover, after adopting the step-by-step method, the heat release of the reaction between ferrous chloride and chlorine is much lower than that of the reaction between chlorine and iron to generate ferrous chloride, and almost no heat is released. Therefore, the temperature of this step is easy to control, and the temperature can be controlled by using an external heat source.
[0080] In step S200, Cl 2 (g)+FeCl 2 (g) →FeCl 3 (g) reaction, which is similar to the above-mentioned FeCl 3 (g) → Cl 2 (g)+FeCl 2 (g) are reverse reactions. Therefore, in step S200, chlorine gas is introduced, which increases the concentration of reactants and shifts the chemical equilibrium toward the positive reaction direction, that is, toward the formation of FeCl 3 (g)
[0081] In addition, during the chlorination process, iron is directly chlorinated into ferric chloride, which requires stronger chlorination conditions. See the analysis in part S100, which can easily lead to the chlorination of other elements in the alloy. In addition, during the chlorination process, iron is continuously volatilized, resulting in constantly changing reaction conditions, making it impossible to obtain relatively stable reaction conditions, which is not conducive to large-scale industrial production.
[0082] S300: The ferric chloride gas is drawn out to react with oxygen to obtain iron oxide and recover chlorine; wherein the reaction temperature is 700-1200° C., and the amount of oxygen introduced is 0.75-1.1 times the volume of the ferric chloride gas.
[0083] The ferric chloride gas is drawn out from the reaction chamber of S200 and reacts with oxygen to obtain iron oxide (i.e., ferric oxide) and recover chlorine gas.
[0084] In the above-mentioned comprehensive treatment method of iron in the iron-containing alloy, by controlling the chlorination conditions, the preferential chlorination of iron in the alloy is achieved, and it is converted into molten ferrous chloride. Then the ferrous chloride is converted into gaseous ferric chloride and volatilized, and cooled to obtain ferric chloride. The ferric chloride is reoxidized to obtain iron oxide and recycle chlorine. The element behavior of iron in the alloy is to convert from a solid alloy into liquid ferrous chloride, then into gaseous ferric chloride, and finally into iron oxide, which realizes the continuity of the process. And in the process of molten ferrous chloride passing through chlorine gasification, the reaction can be well controlled, and then high-quality ferric chloride can be prepared. Recovered chlorine can be used directly or used as chlorine after purification, thereby reducing production costs. The above-mentioned comprehensive treatment method of iron in the iron-containing alloy is simple to operate, has a short process flow, and obtains high-quality iron oxide.
[0085] In some embodiments, it also includes:
[0086] The recovered chlorine gas is introduced into the iron-containing alloy to form the chlorine gas atmosphere.
[0087] The recovered chlorine gas is drawn out from the top of the oxidation reaction chamber and introduced into the iron-containing alloy for repeated use, thereby reducing the cost.
[0088] The present application also provides a comprehensive treatment device for iron in ferroalloys, referring to Figure 1 , including a roasting furnace 100, a separation mechanism 200, a chlorination reaction chamber 300, an oxidation reaction chamber 400 and an iron oxide collection chamber 700.
[0089] The roasting furnace 100 includes a furnace body 120 and a first chlorine gas inlet 110. The furnace body 120 has a receiving cavity for receiving the iron-containing alloy. The first chlorine gas inlet is connected to the receiving cavity, and the mass of the chlorine gas introduced is 0.8 to 1.5 times the mass of the iron-containing alloy. The roasting temperature in the furnace body 120 is 500 to 850°C. The specific shape of the roasting furnace 100 is not limited, such as cylindrical, square, etc. The surface of the furnace body 120 has a temperature control and heat preservation device 130.
[0090] The separation mechanism 200 is communicated with the accommodating chamber to separate the ferrous chloride melt generated by the furnace body 120 .
[0091] The chlorination reaction chamber 300 has a second chlorine gas inlet 310. The chlorination reaction chamber 300 is connected to the separation mechanism 200. The chlorination reaction chamber 300 receives the ferrous chloride melt and reacts with the second chlorine gas to generate ferric chloride gas. In some embodiments, the surface of the chlorination reaction chamber 300 has a first temperature control device 320.
[0092] The oxidation reaction chamber 400 has an oxygen inlet 450 and a chlorine outlet 430. The oxidation reaction chamber 400 is connected to the chlorination reaction chamber 300. The oxidation reaction chamber 400 receives the ferric chloride gas and reacts it with oxygen to obtain iron oxide and recover chlorine. In some embodiments, the surface of the oxidation reaction chamber 400 also has a second temperature control device 440.
[0093] The iron oxide collection chamber 700 is communicated with the oxidation reaction chamber 400 to condense and recover the iron oxide.
[0094] In some specific embodiments, reference Figure 1 The height-to-diameter ratio of the furnace body 120 is controlled at 5:1-15:1, the length-to-diameter ratio of the chlorination reaction chamber 300 is controlled at 5:1-10:1, the height-to-diameter ratio of the reaction zone of the oxidation reaction chamber 400 is controlled at 8:1-15:1, and the height of the chlorine outlet Y-7 is controlled at 15-25 meters.
[0095] The above-mentioned comprehensive treatment device for iron elements in iron-containing alloys is used to implement the above-mentioned comprehensive treatment method for iron elements in iron-containing alloys, and has corresponding beneficial effects, which will not be described in detail.
[0096] In some embodiments, reference Figure 1 and Figure 2 The separation mechanism 200 includes a plurality of connecting pipes 210 evenly distributed on the bottom surface of the furnace body 120, forming a pipeline for separating the ferrous chloride melt; the plurality of connecting pipes 210 each include a first end and a second end opposite to each other; the first end extends into the furnace body 120 and exceeds the bottom of the furnace body 120, and the second end is connected to the chlorination reaction chamber 300; the opening of the first chlorine gas inlet 110 close to the furnace body 120 is located in the area between the first end and the bottom of the furnace body 120; the first chlorine gas inlet 110 and the connecting pipes 210 are alternately distributed.
[0097] The diameter of the connecting tube 210 is relatively small, and for example, the inner diameter of the connecting tube 210 is 1-3 cm. The iron-containing alloy is not easy to enter the chlorination reaction chamber 300 through the connecting tube 210, while the ferrous chloride melt can enter the chlorination reaction chamber 300 through the connecting tube 210. Therefore, the multiple connecting tubes 210 actually play a role in solid-liquid separation.
[0098] Since the first end of the connecting pipe 210 extends above the bottom of the furnace body 120, the ferrous chloride melt above the first end enters the chlorination reaction chamber 300. The ferrous chloride melt remains between the bottom of the furnace body 120 and the end of the first end.
[0099] The first chlorine gas inlet 110 is close to the opening of the furnace body 120, that is, the position where the chlorine gas is introduced. It is located in the area between the first end and the bottom of the furnace body 120, so the chlorine gas will always contact with the ferrous chloride melt, at least with the remaining ferrous chloride melt, to avoid the ferrous chloride melt from entering the chlorination reaction chamber 300 completely, resulting in a waste of the first chlorine gas.
[0100] In some embodiments, reference Figure 1 and Figure 2 The first chlorine gas inlet 110 is inclined downward from the outside of the furnace body 120 to the inside of the furnace body 120 , and the end of the first end of the connecting pipe 210 is provided with a shielding portion 211 for preventing the iron-containing alloy from entering the connecting pipe 210 .
[0101] The iron-containing alloy contains some fine particles, in order to prevent them from clogging the first chlorine gas inlet 110 and the connecting pipe 210. The first chlorine gas inlet 110 is tilted from top to bottom. The first chlorine gas inlet 110 is located at the lowest position close to the opening of the furnace body 120, so as to prevent the iron-containing alloy from entering the first chlorine gas inlet 110 under the action of gravity and causing blockage. A small amount of iron-containing alloy entering the first chlorine gas inlet 110 will be blown out by the chlorine gas.
[0102] The end of the first end of the connecting tube 210 is provided with a shielding portion 211, which directly protects the end of the first end to prevent the iron-containing alloy from falling vertically into the connecting tube 210. There is a gap between the shielding portion 211 and the connecting tube 210 to form a flow channel for the ferrous chloride melt to enter, and the ferrous chloride melt passes through the flow channel and enters the connecting tube 210. Exemplarily, the shielding portion 211 is an umbrella-shaped structure, and the iron-containing alloy falls on the umbrella-shaped structure and slides down. In a more specific embodiment, the flow channel is arranged obliquely upward, and the structure beside the flow channel shields the iron-containing alloy in the horizontal direction, so that the iron-containing alloy is less likely to enter the connecting tube 210.
[0103] In some embodiments, reference Figure 1 and Figure 2 The connecting pipe 210 includes a bending section 212 that bends back and forth along the height direction of the furnace body 120 .
[0104] The bending section 212 is located in the middle of the connecting pipe 210. The bending section 212 is arranged along the height direction of the furnace body 120. The bending section 212 includes a plurality of segments, which are arranged along the height direction and connected end to end in sequence. The bending section 212 forms a connecting vessel structure.
[0105] The communicating vessel structure is located in the middle of the communicating pipe 210. Under the action of gravity, the ferrous chloride melt in the furnace body 120 flows from the first end of the communicating pipe 210, through the communicating vessel structure, and enters the chlorination oxidation reaction chamber 400 from the second end. The bottom of the communicating vessel structure always retains the ferrous chloride melt, which can act as a check valve, and the one-way conduction only allows the ferrous chloride melt to enter the chlorination reaction chamber 300. The gaseous ferric chloride generated in the chlorination reaction chamber 300 or the chlorine gas introduced therein cannot enter the furnace body 120 due to the presence of the ferrous chloride melt at the bottom of the communicating vessel.
[0106] In some embodiments, reference Figure 1 and Figure 2 The parts of the plurality of connecting pipes 210 in the furnace body 120 can be extended and retracted. The depth of the ferrous chloride melt phase in the furnace body 120 is controlled by the height of the extension. For example, the connecting pipe 210 includes a first sleeve in the furnace body 120 and a second sleeve in the furnace body 120, and the first sleeve is nested outside the second sleeve and can move along the axial direction of the second sleeve.
[0107] In some embodiments, reference Figure 1 and Figure 2 , further comprising a top sealing device 500 and a feeding mechanism 600; the top sealing device 500 is located at the top of the furnace body 120, and is used to seal the furnace body 120 to prevent chlorine from escaping. The feeding mechanism 600 comprises an alloy inlet 610, a pre-installed component 620 and an alloy adding inlet 630 which are sequentially arranged from bottom to top at the top of the furnace body 120. The alloy inlet 610 comprises a plurality of insertion channels 611 which are connected to the furnace body 120 through the top sealing device 500. The pre-installed component 620 is funnel-shaped, and its bottom is connected to the side of the alloy inlet 610 away from the furnace body 120. The bottom of the pre-installed component 620 has a first sealed switch 621. The alloy adding inlet 630 is connected to the top of the pre-installed component 620, and the alloy adding inlet 630 has a second sealed switch 631.
[0108] The multiple introduction channels 611 allow the iron-containing alloy to enter the furnace body 120 in multiple streams, and the iron-containing alloy is distributed more evenly in the furnace body 120. In some specific embodiments, the diameter of the introduction channel 611 corresponding to the middle of the furnace body 120 is smaller than the diameter of the introduction channel 611 corresponding to the edge of the furnace body 120. Since the alloy flow velocity in the introduction channel 611 in the middle of the furnace body 120 is relatively high, while the alloy flow velocity in the introduction channel 611 at the edge of the furnace body 120 is relatively low, the diameters of the introduction channels 611 of the two introduction channels 611 are designed as above to balance the total amount of the iron-containing alloy in the introduction channel 611 at the edge of the furnace body 120 and the introduction channel 611 in the middle of the furnace body 120, so that the iron-containing alloy is distributed more evenly in the middle and the edge of the furnace body 120.
[0109] The lower part of the pre-installed component 620 is a small end with a smaller diameter, and the upper part is a large end with a larger diameter. The small end is connected to the alloy inlet 610, and the large end is connected to the alloy addition inlet 630. The pre-installed component 620 serves as a temporary storage mechanism for the iron-containing alloy, ensuring that the flow rate of the iron-containing alloy from the pre-installed component 620 into the alloy inlet 610 is relatively stable. After the first sealed switch 621 is closed, the iron-containing alloy stops entering the alloy inlet 610, and further seals the top of the furnace body 120 to prevent chlorine from escaping.
[0110] The number of the alloy adding inlets 630 is not limited, such as 1, 2 or more. The second sealed switch 631 is opened, and the iron-containing alloy is added to the pre-assembled component 620 from the alloy adding inlet 630 .
[0111] The conditions for controlling the chlorination of the molten salt in the roasting furnace 100 are: the chlorination temperature is 600-800°C, and the stacking height of the alloy can be controlled to be not less than 0.5m through the feeding mechanism 600 during the chlorination process. In addition, chlorine gas is introduced from the bottom of the stacked alloy during the chlorination process.
[0112] In some embodiments, reference Figure 1 and Figure 3 , the second chlorine gas inlet 310 includes a side inlet 311 and a bottom inlet 312. The side inlet 311 is located at the lower side of the chlorination reaction chamber 300 away from the oxidation reaction chamber 400, and is evenly distributed in the vertical direction (for example, the number of the side inlets 311 is 3). The bottom inlet 312 is located at the bottom of the chlorination reaction chamber 300, and is evenly distributed in an area extending 2 / 3 along the length direction from one side of the oxidation reaction chamber 400 (for example, the number of the bottom inlet 312 is 7). The comprehensive treatment device also includes a one-way air intake mechanism 330 that conducts from the chlorination reaction chamber 300 to the oxidation reaction chamber 400.
[0113] The above-mentioned arrangement of the side air inlet 311 and the bottom air inlet 312 is far away from the oxidation reaction chamber 400, so that chlorine gas is not easy to enter the oxidation reaction chamber 400, thereby reducing the amount of chlorine gas entering the oxidation reaction chamber 400.
[0114] The one-way air inlet mechanism 330 (such as a one-way valve) can prevent oxygen, ferric chloride gas and recovered chlorine gas from flowing back into the chlorination reaction chamber 300 .
[0115] The conditions for secondary chlorination of molten salt in the chlorination reaction chamber 300 to produce ferric chloride gas are: chlorination temperature 500-800°C, the height of the molten salt is controlled to be not less than 0.2m during the chlorination process, and chlorine gas is introduced from the side air inlet 311 and the bottom air inlet 312 during the chlorination process.
[0116] In some embodiments, reference Figure 1 and Figure 3 The oxygen inlet 450 extends from the side into the interior of the oxidation reaction chamber 400 and is located at a height of 1 / 2-2 / 3 from the top of the chamber; the oxidation reaction chamber 400 also includes an online monitoring device 410 for chlorine and oxygen content and a ferric chloride gas supplement port 420.
[0117] The chlorine and oxygen contents in the chamber are monitored by the chlorine and oxygen content online monitoring device 410. The conditions for the oxidation of ferric chloride gas by oxygen to produce iron oxide and chlorine are: oxidation temperature 700-1100°C, close monitoring of the chlorine and oxygen contents in the gas during the oxidation process, when the oxygen content is higher than 2%, stop adding oxygen, and simultaneously add ferric chloride gas from the ferric chloride gas adding port 420 until the oxygen content is less than or equal to 2%, and then introduce oxygen.
[0118] In some embodiments, reference Figure 1 and Figure 3 The chlorine gas outlet 430 is connected to the furnace body 120. The chlorine gas outlet 430 is disposed at the top of the oxidation reaction chamber 400.
[0119] In some embodiments, reference Figure 1 and Figure 4 The iron oxide collection chamber 700 includes a first discharge chamber 710, a third sealed switch 730, a second discharge chamber 720 and a fourth sealed switch 740 which are arranged in sequence from top to bottom.
[0120] The purpose of the first discharge chamber 710, the third sealed switch 730, the second discharge chamber 720 and the fourth sealed switch 740 is to discharge the iron oxide without affecting the reaction in the furnace. It is similar to when the roasting furnace 100 is charged. That is, the generated iron oxide naturally falls into the first discharge chamber 710, and the third sealed switch 730 and the fourth sealed switch 740 are in a closed state. Open the third sealed switch 730 and close the fourth sealed switch 740, and the iron oxide falls into the second discharge chamber 720. Close the third sealed switch 730 and open the fourth sealed switch 740, and the iron oxide is released from the reactor.
[0121] Embodiment 1:
[0122] use Figure 1 The comprehensive treatment device for iron in ferrous alloys shown is provided under the following conditions:
[0123] Add 1 kg of ferrous alloy to Figure 1 In the feeding mechanism 600 shown in the figure, 1 kg of ferrous alloy is added into the roasting furnace 120 through the feeding mechanism 600. The temperature in the furnace reaches 600°C through the temperature control and heat preservation device 130, and chlorine is immediately introduced into the furnace through the first chlorine gas inlet 110. The amount of chlorine added is 1.1 times the mass of the ferrous alloy. When ferrous chloride melt flows into the furnace, the chlorine gas is added to the furnace. Figure 1 When the chlorination reaction chamber 300 of the device is opened, 1 kg of alloy already added to the device 600 is added to Figure 1 In the device 600 shown in the figure, chlorine is continuously introduced into the furnace through the first chlorine inlet 110. The amount of chlorine added in this stage is 1 times the mass of the second batch of ferrous alloy added. During the reaction, the roasting temperature is maintained at 600°C by the temperature control and heat preservation device 130. The obtained ferrous chloride melt sample is as follows Figure 5 shown.
[0124] The temperature in the furnace is brought to 650°C by the temperature control and heat preservation device 130, and chlorine is introduced into the chlorination reaction chamber 300 through the side air inlet 311 and the bottom air inlet 312. The amount of chlorine introduced is 0.28 times the mass of the ferrous chloride melt (the specific amount is determined based on the height of the melt in the chlorination reaction chamber 300), so that the iron salt in the melt is converted into ferric chloride and volatilized. The obtained ferric chloride sample is as follows Figure 6 shown.
[0125] The ferric chloride gas obtained in the chlorination reaction chamber 300 is led out through 330 and enters Figure 1 The oxidation reaction chamber 400 shown in FIG. 1 is provided with oxygen through an oxygen inlet 450, wherein the amount of oxygen introduced is 0.9 times the volume of the ferric chloride gas. The temperature in the furnace is set to 1000° C. through a second temperature control device 440 to obtain iron oxide and recover chlorine. The test results of the obtained iron oxide sample are shown in FIG. Figure 7 and Figure 8 As shown, the obtained iron oxide product has uniform particle size distribution and a purity of 99.99%. The recovered chlorine is discharged through the chlorine outlet 430, and after compression and liquefaction, the purity of the obtained liquid chlorine reaches 99.9%.
[0126] Embodiment 2:
[0127] The reaction equipment is the same as in Example 1, and the conditions are as follows:
[0128] Add 1 kg of ferrous alloy to Figure 1 In the feeding mechanism 600 shown in the figure, 1 kg of ferrous alloy is added into the roasting furnace 120 through the feeding mechanism 600. The temperature in the furnace reaches 650°C through the temperature control and heat preservation device 130, and chlorine is immediately introduced into the furnace through the first chlorine inlet 110. The amount of chlorine added is 1 times the mass of the ferrous alloy. When ferrous chloride melt flows into the furnace, the chlorine gas is added to the furnace. Figure 1 When the chlorination reaction chamber 300 of the device is opened, 1 kg of alloy already added to the device 600 is added to Figure 1 In the device 600 shown, chlorine is continuously introduced into the furnace through the first chlorine inlet 110. The amount of chlorine added in this stage is 1 times the mass of the second batch of ferrous alloy added. During the reaction, the roasting temperature is maintained at 650°C by the temperature control and insulation device 130.
[0129] The temperature in the furnace reaches 700° C. through the temperature control and insulation device 130, and chlorine gas is introduced into the chlorination reaction chamber 300 through the side air inlet 311 and the bottom air inlet 312. The amount of chlorine gas introduced is 0.3 times the mass of the ferrous chloride melt (the specific amount is determined based on the height of the melt in the chlorination reaction chamber 300), so that the iron salt in the melt is converted into ferric chloride and volatilized.
[0130] The ferric chloride gas obtained in the chlorination reaction chamber 300 is led out through 330 and enters Figure 1 In the oxidation reaction chamber 400 shown, oxygen is introduced into the oxidation reaction chamber 400 through the oxygen inlet 450, and the amount of oxygen introduced is 1 times the volume of the ferric chloride gas. The temperature in the furnace reaches 1100° C. through the second temperature control device 440, and iron oxide and recovered chlorine are obtained, and the purity of the iron oxide reaches 99.99%. The recovered chlorine is discharged through the chlorine outlet 430, and after compression and liquefaction, the purity of the obtained liquid chlorine reaches 99.8%.
[0131] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A comprehensive treatment method for iron in ferroalloys, It is characterized in that The following steps are involved: The iron-containing alloy is roasted in a chlorine atmosphere to obtain a ferrous chloride melt and solid slag, and the ferrous chloride melt is separated; wherein the mass of the chlorine is 0.8 to 1.5 times the mass of the iron-containing alloy, and the roasting temperature is 500 to 850° C.; Chlorine is introduced into the ferrous chloride melt to carry out a chlorination reaction, so that the ferrous chloride melt is converted into ferric chloride gas; wherein the temperature of the chlorination reaction is 400-700° C., and the amount of chlorine introduced is 0.25-0.35 times the mass of the ferrous chloride melt; The ferric chloride gas is drawn out to react with oxygen to obtain iron oxide and recover chlorine; wherein the reaction temperature is 700-1200° C., and the amount of oxygen introduced is 0.75-1.1 times the volume of the ferric chloride gas.
2. The comprehensive treatment method according to claim 1, It is characterized in that Also includes: The recovered chlorine gas is introduced into the iron-containing alloy to form the chlorine gas atmosphere.
3. A comprehensive treatment device for iron in ferroalloys, It is characterized in that include: A roasting furnace, comprising a furnace body and a first chlorine gas inlet, wherein the furnace body has a containing cavity for containing the iron-containing alloy, the first chlorine gas inlet is connected to the containing cavity, and the mass of the chlorine gas introduced is 0.8 to 1.5 times the mass of the iron-containing alloy; the roasting temperature in the furnace body is 500 to 850°C; A separation mechanism, connected to the accommodating chamber, for separating the ferrous chloride melt generated by the furnace body; a chlorination reaction chamber having a second chlorine gas inlet, the chlorination reaction chamber being in communication with the separation mechanism, the chlorination reaction chamber receiving the ferrous chloride melt and reacting the ferric chloride melt with the second chlorine gas to generate ferric chloride gas; An oxidation reaction chamber has an oxygen inlet and a chlorine outlet; the oxidation reaction chamber is connected to the chlorination reaction chamber, the oxidation reaction chamber receives the ferric chloride gas and reacts it with oxygen to obtain ferric oxide and recover chlorine; The iron oxide collection chamber is connected to the oxidation reaction chamber to collect and recycle the iron oxide.
4. The integrated processing device according to claim 3, It is characterized in that The separation mechanism includes a plurality of connecting pipes evenly distributed on the bottom surface of the furnace body, forming a pipeline for separating the ferrous chloride melt; the plurality of connecting pipes each include a first end and a second end opposite to each other; the first end extends into the furnace body and exceeds the bottom of the furnace body, and the second end is connected to the chlorination reaction chamber; The opening of the first chlorine gas inlet close to the furnace body is located in the area between the first end and the bottom of the furnace body; the first chlorine gas inlet and the connecting pipe are alternately distributed.
5. The integrated processing device according to claim 4, It is characterized in that The first chlorine gas inlet is arranged to be inclined downward from outside the furnace body to inside the furnace body, and a shielding portion for preventing the iron-containing alloy from entering the connecting pipe is provided at the end of the first end of the connecting pipe.
6. The integrated processing device according to claim 4, It is characterized in that The connecting pipe includes a bending section that bends back and forth along the height direction of the furnace body; Portions of the plurality of connecting pipes within the furnace body are retractable.
7. The integrated processing device according to claim 3, It is characterized in that It also includes a top sealing device and a feeding mechanism; The top sealing device is located at the top of the furnace body and is used to seal the furnace body; The feeding mechanism comprises: An alloy introduction port, comprising a plurality of introduction channels connected to the furnace body through the top sealing device; The pre-installed component is funnel-shaped, and the bottom is connected to the alloy inlet away from the furnace body; the bottom of the pre-installed component has a first sealed switch; The alloy adding port is communicated with the top of the preassembled component, and the alloy adding port is provided with a second sealed switch.
8. The integrated processing device according to claim 3, It is characterized in that The second chlorine gas inlet includes a side inlet and a bottom inlet; The side air inlets are located at the lower part of the side of the chlorination reaction chamber away from the oxidation reaction chamber and are evenly distributed vertically; The bottom air inlet is located at the bottom of the chlorination reaction chamber and is evenly distributed in an area extending 2 / 3 along the length direction from one side of the oxidation reaction chamber; The comprehensive treatment device also includes a one-way air intake mechanism that connects the chlorination reaction chamber to the oxidation reaction chamber.
9. The integrated processing device according to claim 4, It is characterized in that The oxygen inlet extends from the side into the interior of the oxidation reaction chamber and is located at a height of 1 / 2-2 / 3 from the top of the chamber.
10. The integrated processing device according to any one of claims 4 to 9, It is characterized in that The oxidation reaction chamber also includes an online monitoring device for chlorine and oxygen content and a ferric chloride gas supply port.