Preparation method and application of Ti4O7 doped Cu electrode material
By doping Cu powder in Ti4O7 electrode and using sol-hydrothermal method and vacuum plasma sintering technology, an efficient Ti4O7-doped Cu electrode material was prepared, which solved the problem of low charge transfer rate at the interface of the original Ti4O7 electrode, significantly improving the The degradation effect of carbamazepine.
Patent Information
- Application Number
- CN202411336758.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
The original Ti4O7 electrode has a low interfacial charge transfer rate, resulting in poor electrochemical properties and degradation of pollutants.
Cu powder is doped in Ti4O7 powder, Cu doped material powder is prepared by sol-hydrothermal method, and mixed with Ti4O7 in powder form and sintered in a vacuum plasma sintering furnace to prepare Ti4O7-doped Cu electrode material to improve its Oxygen evolution potential and degradation capacity.
The doped electrode material has a higher oxygen evolution potential and can generate more hydroxyl radicals, which significantly improves the degradation effect on the pollutant carbamazepine, with a degradation rate of 91.21%.
Smart Images

Figure CN119080156A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrode materials, and in particular relates to a preparation method and application of a Ti4O7 Cu-doped electrode material. Background Art
[0002] Ti4O7 has been widely used in electrode materials, battery loading materials and catalyst coating materials for advanced oxidation treatment of organic wastewater. Some studies have used Ti4O7 as an electrode in the electrochemical oxidation process of difficult-to-degrade printing and dyeing wastewater and found that it has good degradation activity and stability.
[0003] However, the original Ti4O7 has a low interfacial charge transfer rate. Therefore, it is necessary to modify the Ti4O7 electrode to improve its electrochemical properties and its degradation of pollutants. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a Ti4O7 doped Cu electrode material and its application in view of the deficiencies of the above-mentioned prior art. The method prepares an electrode material by doping Cu powder in Ti4O7 powder. The doped electrode has a higher oxygen evolution potential than a pure Ti4O7 electrode, thereby generating more hydroxyl free radicals, which can improve the electrochemical properties and has a good degradation effect on carbamazepine in pollutants.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a Ti4O7-doped Cu electrode material, the method comprising:
[0006] S1. Add CuCl2 to deionized water and stir at room temperature for 1 h to obtain a CuCl2 aqueous solution;
[0007] S2, mixing the CuCl2 aqueous solution and the NaOH aqueous solution obtained in S1 and ultrasonically dispersing them for 30 minutes to obtain a mixed substance;
[0008] S3, adding anhydrous ethanol to the mixed substance obtained in S2, and performing a hydrothermal reaction at a temperature of 180° C. for 24 hours to obtain a hydrothermal reaction product;
[0009] S4, naturally cooling the hydrothermal product in S3 to room temperature, centrifuging, washing the precipitate with anhydrous ethanol three times, then washing with deionized water three times, and drying at 80°C for 12h to obtain a dried substance;
[0010] S5, grinding the dried material obtained in S4 for 15 minutes to obtain Cu-doped material powder;
[0011] S6. After the Cu-doped material powder and Ti4O7 powder obtained in S5 are shaken and mixed evenly, they are placed in a graphite mold, sintered in a dual-power vacuum plasma sintering furnace, and then taken out to obtain a Ti4O7-doped Cu electrode material; the sintering system is: under a vacuum condition with a pressure of 5 MPa, the temperature is increased from room temperature to 600°C at a heating rate of 114°C / min, and then from 600°C to 1000°C at a heating rate of 50°C / min, and then from 1000°C to 1100°C at a heating rate of 25°C / min, and the temperature is maintained at a constant temperature for 20 minutes, and then naturally cooled to room temperature under a pressure of 5 MPa.
[0012] Preferably, the concentration of the CuCl2 aqueous solution in S1 is 0.2M.
[0013] Preferably, the concentration of the NaOH aqueous solution in S2 is 1 M; the volume ratio of the CuCl2 aqueous solution to the NaOH aqueous solution is 1:1.
[0014] Preferably, the volume of the anhydrous ethanol in S3 is equal to the volume of the NaOH aqueous solution in S2.
[0015] Preferably, the particle size of the Cu-doped material powder in S5 is 1.28 μm to 2.30 μm.
[0016] Preferably, the mass of the Cu-doped material powder in S6 is 2% to 4% of the mass of the Ti4O7 powder.
[0017] The present invention also provides application of the Ti4O7-doped Cu electrode material prepared by the above-mentioned preparation method, wherein the Ti4O7-doped Cu electrode material is used for degrading carbamazepine.
[0018] Preferably, the degradation rate of carbamazepine by the Ti4O7 doped Cu electrode material in 60 min is 91.21%.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] The present invention uses a sol-hydrothermal method to prepare a Cu-doped material powder, and then the two materials (Cu-doped material powder and Ti4O7) are directly mixed in the form of powder and then sintered in a dual-power vacuum plasma sintering furnace. The step-by-step preparation can ensure that the two materials reach the required purity, and Ti4O7 powder is mainly used, and a small amount of Cu-doped material powder is doped in the Ti4O7 powder, so that the advantages of Ti4O7 itself can be brought into play, and the advantages of Cu-doped material powder can also be brought into play. In terms of performance, the prepared electrode material is directly sintered from powder, the two materials are tightly combined, there is no problem of falling off during the reaction, and the stability is more advantageous. The anode material prepared by doping Cu powder in Ti4O7 powder of the present invention has a higher oxygen evolution potential than the pure Ti4O7 electrode after doping, thereby generating more hydroxyl radicals, can improve electrochemical characteristics, and has a good degradation effect on carbamazepine in pollutants.
[0021] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is an electron microscope picture of the electrode material of Ti4O7 doped with Cu doped material powder (doping ratio is 4%) prepared in Example 1 of the present invention.
[0023] Figure 2 This is the XRD spectrum of the electrode material of the Ti4O7 doped Cu doped material powder prepared in Example 1 of the present invention.
[0024] Figure 3 This is a comparison chart of the carbamazepine degradation effects of the electrode material of the Ti4O7 doped Cu doped material powder (doping ratio is 4%) prepared in Example 1 of the present invention, the Ti4O7 doped Cu electrode prepared by the other two preparation methods (ball milling method and impregnation method) and the pure Ti4O7 electrode.
[0025] Figure 4 This is a comparison chart of the degradation effects of Ti4O7-doped Cu-doped material powder (different doping ratios = 2%, 3%, 4%) on carbamazepine prepared in Example 1 of the present invention.
[0026] Figure 5 It is a linear sweep voltammogram of the electrode material of Ti4O7 doped with Cu doped material powder (doping ratio is 4%) prepared in Example 1 of the present invention.
[0027] Figure 6 It is a comparative electrochemical impedance spectrum of the Ti4O7 doped Cu doped material powder (doping ratio is 4%) prepared in Example 1 of the present invention and the pure Ti4O7 electrode. DETAILED DESCRIPTION
[0028] Example 1
[0029] The preparation method of the electrode material of Ti4O7 doped with Cu in this embodiment is as follows:
[0030] S1. Add CuCl2 to deionized water and stir at room temperature for 1 h to obtain a 0.2 M CuCl2 aqueous solution;
[0031] S2, mixing the CuCl2 aqueous solution obtained in S1 and an equal volume of a 1M NaOH aqueous solution and ultrasonically dispersing them for 30 minutes to obtain a mixed substance;
[0032] S3, adding anhydrous ethanol to the mixed substance obtained in S2, and performing a hydrothermal reaction at a temperature of 180° C. for 24 hours to obtain a hydrothermal reaction product;
[0033] S4, naturally cooling the hydrothermal product in S3 to room temperature, centrifuging, washing the precipitate with anhydrous ethanol three times, then washing with deionized water three times, and drying at 80°C for 12h to obtain a dried substance;
[0034] S5, grinding the dried material obtained in S4 for 15 minutes to obtain a Cu-doped material powder with a particle size of 1.28 μm to 2.30 μm;
[0035] S6, after the Cu-doped material powder and Ti4O7 powder obtained in S5 are shaken and mixed evenly, they are placed in a graphite mold, sintered in a dual-power vacuum plasma sintering furnace, and then taken out to obtain a Ti4O7-doped Cu electrode material; the sintering system is: under a vacuum condition with a pressure of 5MPa, the temperature is increased from room temperature to 600°C at a heating rate of 114°C / min, then from 600°C to 1000°C at a heating rate of 50°C / min, and then from 1000°C to 1100°C at a heating rate of 25°C / min, and the temperature is kept constant for 20min, and then naturally cooled to room temperature under a pressure of 5MPa;
[0036] This embodiment also provides an application of the Ti4O7-doped Cu electrode material prepared by the above-mentioned preparation method, wherein the Ti4O7-doped Cu electrode material is used to degrade carbamazepine.
[0037] like Figure 1 (b) shows the surface of a pure Ti4O7 electrode (the sintering method is the same as step S6 of this embodiment). It can be seen that the surface is somewhat rough and there are gaps between the particles. Figure 1 (a) shows the electrode surface of the Ti4O7 doped Cu electrode material prepared in this example. It can be seen that the surface is smooth and there are still gaps between the particles.
[0038] The XRD patterns of the pure Ti4O7 electrode and the Ti4O7 / Cu electrode (the electrode material electrode doped with Cu prepared in this embodiment) are as follows: Figure 2 As shown, all characteristic diffraction peaks are observed for the pure Ti4O7 electrode. There is not much difference between the diffraction peaks of the Ti4O7 / Cu electrode and the pure Ti4O7 electrode, but the intensity of the diffraction peaks is greatly reduced.
[0039] The comparison of the degradation effects of pure Ti4O7 electrode and Ti4O7 / Cu electrode (electrode material electrode doped with Cu by different preparation processes) on carbamazepine is shown in the figure below. Figure 3 As shown, it can be seen that under the comparison of different processes, the degradation ability of this embodiment is still at a superior level.
[0040] Comparison of the degradation effects of Ti4O7 / Cu electrodes (different doping ratios = 2%, 3%, 4%) on carbamazepine Figure 4 As shown, it can be seen that the degradation ability changes under different doping ratios, and the degradation effect is best when the doping ratio is 4%. (The doping ratio is the mass ratio of Cu doped material powder and Ti4O7 powder)
[0041] The linear sweep voltammograms of the pure Ti4O7 electrode and the Ti4O7 / Cu electrode (the electrode material electrode doped with Cu prepared in this example) are shown in FIG. Figure 5 As shown, the oxygen evolution potential of Ti4O7 is 2.099 V, while the oxygen evolution potential of Ti4O7 doped with Cu is 2.36 V. The high oxygen evolution potential is conducive to the generation of hydroxyl radicals and inhibits the oxygen evolution side reaction on the electrode surface.
[0042] The electrochemical impedance spectra of the pure Ti4O7 electrode and the Ti4O7 / Cu electrode (the electrode material electrode doped with Cu prepared in this example) are as follows: Figure 6 As shown, it can be clearly seen in the EIS graph that the EIS radius of the Ti4O7 doped Cu electrode is larger than that of the Ti4O7 electrode, which means that its interface charge transfer resistance has changed.
[0043] The Ti4O7 doped Cu electrode prepared in this experiment was used to study the degradation of carbamazepine. Figure 3As shown, the degradation rates of carbamazepine for pure Ti4O7 electrode and Ti4O7 / Cu electrode (Ti4O7 doped with Cu electrode prepared in this embodiment) were 91.21% and 39.3% respectively in 60 min. It can be seen that the doped Ti4O7 electrode is better than the undoped electrode and the degradation of Ti4O7 doped with Cu electrode is faster. This is because the oxygen evolution potential of Ti4O7 / Cu electrode is higher than that of Ti4O7, which is conducive to the generation of hydroxyl radicals and the degradation of carbamazepine. Experimental conditions: 100mL of 10mg / L carbamazepine aqueous solution was measured, 1.4204g of Na2SO4 electrolyte was added, and the mixture was poured into the electrolytic cell. Ti4O7 and Ti4O7 / Cu were used as anodes, respectively, and pure titanium mesh of the same size with a surface polished with 400cc of sandpaper was used as cathode. A double electrode system with a constant current density of 20mA / cm 2 , magnetic stirring rate 750r / min, oxidation at room temperature for 60min.
[0044] This example also compares the electrode preparation method of this example with two other processes (ball milling method and immersion method).
[0045] Comparative Example 1
[0046] Ball milling method: Put Ti4O7 powder and CuO into a ball mill, add 20 quartz beads with a diameter of 5mm and 40 quartz beads with a diameter of 2mm into the ball mill, seal it and put it into a ball mill. Ball mill for 4 hours at a speed of 500r / min. After the ball milling is completed, take out the powder, wash it with water five times to remove the unreacted ions, and then dry it at 80℃ for 6 hours. After drying, 2g of Ti4O7 doped Cu powder is obtained. Then place it in a graphite mold and send it to a dual-power vacuum plasma sintering furnace for sintering at 1100℃ for 20 minutes. After the electrode is cooled, it is polished to obtain a solid disc electrode (diameter: 2cm, thickness: 1mm), and then the electrode is activated under low current conditions.
[0047] Comparative Example 2
[0048] Impregnation method: Take 2g of Ti4O7 powder, put the powder into a cylindrical graphite mold with a diameter of 2cm, and place it in a vacuum plasma sintering furnace to sinter it to obtain a Ti4O7 electrode sheet with a diameter of 2cm. The Ti4O7 electrode is treated with vacuum plasma. The discharge power of the vacuum plasma treatment is 100W, the treatment gas is argon (Ar) gas, and the treatment time is 30min to obtain a defective Ti4O7 electrode. Immerse the defective Ti4O7 electrode sheet in 50mL of deionized water and ultrasonicate at room temperature for 1h. Then add 0.4g of Cu(NO3)2 powder to the deionized water and stir for 12h to allow the defective Ti4O7 electrode to fully absorb Cu ions. Then take out the electrode, wash it with deionized water, and freeze-dry it for 24h. The dried electrode is placed in a 5% H2 / Ar mixed atmosphere at 5℃·min -1 The heating rate was set at 200℃ for 2h and the obtained electrode sheet was named Cu / Ti4O7.
[0049] However, comparative experiments show that the degradation efficiency of carbamazepine by ball milling in Comparative Example 1 is 31%, the degradation efficiency of carbamazepine by immersion method in Comparative Example 2 is 68.5%, and the degradation efficiency of carbamazepine by Example 1 is 91.21%.
[0050] The preparation method of this embodiment first uses the sol-hydrothermal method to prepare the Cu doped material powder, and then directly mixes the two materials (Cu doped material powder and Ti4O7) in the form of powder and evenly sintered them in a dual-power vacuum plasma sintering furnace. The step-by-step preparation can ensure that the two materials reach the required purity, and Ti4O7 powder is mainly used, and a small amount of Cu doped material powder is doped in the Ti4O7 powder, so that the advantages of Ti4O7 itself can be brought into play, and the advantages of Cu doped material powder can also be brought into play. In terms of performance, the prepared electrode material is directly sintered from powder, the two materials are tightly combined, there is no problem of falling off during the reaction, and the stability is more advantageous.
[0051] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a Ti4O7-doped Cu electrode material, characterized in that: The method is: S1. Add CuCl2 to deionized water and stir at room temperature for 1 h to obtain a CuCl2 aqueous solution; S2, mixing the CuCl2 aqueous solution and the NaOH aqueous solution obtained in S1 and ultrasonically dispersing them for 30 minutes to obtain a mixed substance; S3, adding anhydrous ethanol to the mixed substance obtained in S2, and performing a hydrothermal reaction at a temperature of 180° C. for 24 hours to obtain a hydrothermal reaction product; S4, naturally cooling the hydrothermal product in S3 to room temperature, centrifuging, washing the precipitate with anhydrous ethanol three times, then washing with deionized water three times, and drying at 80°C for 12h to obtain a dried substance; S5, grinding the dried material obtained in S4 for 15 minutes to obtain Cu-doped material powder; S6. After the Cu-doped material powder and Ti4O7 powder obtained in S5 are shaken and mixed evenly, they are placed in a graphite mold, sintered in a dual-power vacuum plasma sintering furnace, and then taken out to obtain a Ti4O7-doped Cu electrode material; the sintering system is: under a vacuum condition with a pressure of 5 MPa, the temperature is increased from room temperature to 600°C at a heating rate of 114°C / min, and then from 600°C to 1000°C at a heating rate of 50°C / min, and then from 1000°C to 1100°C at a heating rate of 25°C / min, and the temperature is maintained at a constant temperature for 20 minutes, and then naturally cooled to room temperature under a pressure of 5 MPa.
2. The method for preparing a Ti4O7-doped Cu electrode material according to claim 1, characterized in that: The concentration of the CuCl2 aqueous solution in S1 is 0.2M.
3. The method for preparing a Ti4O7-doped Cu electrode material according to claim 1, characterized in that: The concentration of the NaOH aqueous solution in S2 is 1 M; the volume ratio of the CuCl2 aqueous solution to the NaOH aqueous solution is 1:
1.
4. The method for preparing a Ti4O7-doped Cu electrode material according to claim 1, characterized in that: The volume of the anhydrous ethanol described in S3 is equal to the volume of the NaOH aqueous solution described in S2.
5. The method for preparing a Ti4O7-doped Cu electrode material according to claim 1, characterized in that: The particle size of the Cu doped material powder described in S5 is 1.28 μm to 2.30 μm.
6. The method for preparing a Ti4O7-doped Cu electrode material according to claim 1, characterized in that: The mass of the Cu-doped material powder in S6 is 2% to 4% of the mass of the Ti4O7 powder.
7. An application of a Ti4O7 doped Cu electrode material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The Ti4O7 doped Cu electrode material is used for degrading carbamazepine.
8. The use according to claim 7, characterized in that: The degradation rate of carbamazepine by the Ti4O7-doped Cu electrode material in 60 minutes is 91.21%.