Geopolymer concrete mix proportion for enhancing mechanical property of concrete by adopting carbon nanotubes and preparation method of geopolymer concrete mix proportion
By introducing carbon nanotubes into geopolymer concrete, forming nanodispersion liquid and mixing with other materials, the problems of insufficient mechanical properties of geopolymer concrete and unused industrial waste are solved, and high toughness and compactness are achieved. Construction in the field of road traffic.
Patent Information
- Application Number
- CN202411309577.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, nanomaterials are less used in geopolymer concrete, resulting in the failure to effectively improve their mechanical properties and industrial wastes to be effectively utilized, which affects the sustainable development of materials and production costs. .
Carbon nanotubes are used as nano-scale fibers with excellent performance. Through specific mixing ratios and preparation methods, it includes stirring carbon nanotube powder into nanodispersion and mixing with other materials to form enhanced geopolymer concrete and improve its mechanical properties. and compactness.
It significantly improves the compressive and tensile strength of ground polymer concrete, reduces the number and length of cracks, realizes the resource utilization of industrial waste, reduces production costs, and is suitable for construction in the field of road transportation.
Smart Images

Figure CN119080450A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of novel building materials, and in particular to a geopolymer concrete mix ratio and a preparation method thereof that utilizes carbon nanotubes to enhance the mechanical properties of concrete. Background Art
[0002] The concept of geopolymer was first proposed by the Frenchman Davidovits in 1978. It is an inorganic aluminosilicate compound with ceramic-like properties. Its development originated from the research results of cement hardening mechanism. It is an inorganic substance generated by chemical reaction under appropriate temperature conditions after appropriate process treatment, which is made of silicon-alumina materials rich in silicon, aluminum and oxygen as the main elements. Compared with ordinary Portland cement, geopolymer has excellent mechanical properties, acid and alkali resistance, high temperature resistance, and metal ion fixing performance. Its main performance is better than traditional cement, and it is the only choice to replace cement. It can be seen that the development of geopolymer to replace ordinary Portland cement has important scientific significance and practical engineering value.
[0003] In recent years, nanomaterials have been used to prepare cement-based materials with high strength and toughness. Carbon nanotubes are nanomaterials made of layered graphite with perfect hexagonal structure and hollow tube shape. Multi-walled carbon nanotubes are a type of carbon nanotubes with excellent physical and mechanical properties and relatively low cost, and are often used to reinforce cement-based composites. A large number of studies have shown that multi-walled carbon nanotubes can improve the mechanical and durability properties of cement-based materials by filling the micropores of cement-based materials, optimizing the microstructure of cement-based materials, and reducing the internal defects of cement-based materials, but the application of nanomaterials in geopolymer concrete is very rare. Summary of the invention
[0004] The purpose of the present invention is to provide a geopolymer concrete containing carbon nanotubes and a preparation method thereof. The carbon nanotube is a nanometer-scale fiber with excellent performance. Its good mechanical and physical properties can improve the mechanical properties of geopolymer concrete.
[0005] Table 1 shows the chemical composition of fly ash (%) raw materials <![CDATA[SiO2(wt%)]]> <![CDATA[Al2O3(wt%)]]> CaO(wt%) MgO(wt%) <![CDATA[Fe2O3(wt%)]]> <![CDATA[K2O(wt%)]]> <![CDATA[SO3(wt%)]]> Others(wt%) Fly ash 52.31 28.59 3.21 2.05 6.22 1.62 1.79 3.41 Table 2 shows the chemical composition of the mineral powder raw materials CaO(wt%) <![CDATA[SiO2(wt%)]]> MgO(wt%) <![CDATA[Fe2O3(wt%)]]> <![CDATA[Al2O3(wt%)]]> <![CDATA[SO3(wt%)]]> Others(wt%) Fly ash 34 34.5 6.01 1.03 17.7 1.64 8.03
[0006] Table 3 shows the chemical composition of sodium hydroxide
[0007] name Relative molecular weight content / % shape NaOH 142.04 96 White translucent crystalline solid
[0008] Table 4 shows the chemical composition of water glass
[0009] name Density Kg / m3 <![CDATA[Na2O content %]]> <![CDATA[SiO2 content %]]> Modulus Baume (Be) Water Glass 1366 8.53 26.98 3.3 3.3
[0010] The invention is also characterized in that the particle size of natural crushed stone is 5mm to 20mm, the fineness modulus of sand is 3.01, and the apparent density is 2503Kg / m 3 The carbon nanotubes are powdered multi-walled carbon nanotubes with a length of 15-30 μm, a diameter of 3-15 nm, a purity of not less than 98%, and a specific surface area of not less than 250 m2 / g.
[0011] A geopolymer concrete mix ratio for carbon nanotube-enhanced concrete mechanical properties and a preparation method thereof include the following steps:
[0012] (1) According to the designed mix ratio, weigh the following materials by weight, including mineral powder 262.9 kg / m 3 ; Fly ash 394.3Kg / m 3 ;Sand 390.09Kg / m 3 ; Crushed stone 910.2Kg / m 3 ; Water glass 165Kg / m 3 ; Sodium hydroxide 24.24Kg / m 3 ; Water 395.5Kg / m 3 ; Carbon nanotube doping 0-0.98Kg / m 3 , water-binder ratio is 0.35;
[0013] (2) further pouring the solid raw materials in (1) into a mixer in order and stirring for 90 seconds to obtain an initial mixture;
[0014] (3) Before the carbon nanotube powder is poured into the blender, 200 ml of water is added to stir it into a nano-dispersion liquid, and ultrasonic vibration is performed for 30 minutes. The remaining water is mixed with weighed NaOH and water glass to form an alkaline excitation solution.
[0015] (4) further pouring the weighed solution into a mixer and stirring for 120 seconds to obtain a final geopolymer concrete mixture;
[0016] (5) further pouring the geopolymer concrete mixture into a triple mold of 100 mm×100 mm×100 mm;
[0017] (6) Further, the mold filled with concrete is placed on a vibration table and vibrated for 60 seconds to make it dense;
[0018] (7) The specimens were further cured at room temperature for 24 hours and then demolded. The molded specimens were placed in a standard curing box with a temperature of 20°C ± 2°C and a humidity of ≥ 95% for curing. After curing for 28 days, a reinforced geopolymer concrete doped with carbon nanotubes was obtained.
[0019] The geopolymer concrete mix ratio and preparation method thereof using carbon nanotubes to enhance the mechanical properties of concrete have at least the following beneficial effects:
[0020] 1) In the present invention, a large amount of fly ash is added to prepare geopolymer concrete, which can realize the resource utilization of industrial waste, reduce the impact on natural resources, reduce production costs, and meet the requirements of sustainable development.
[0021] 2) The incorporation of an appropriate amount of carbon nanotubes in the present invention can improve the mechanical properties, make it have higher toughness, significantly increase its compressive and tensile strength, and significantly reduce the number and length of cracks.
[0022] 3) Before the carbon nanotube powder is poured into the blender, 200 ml of water is added to stir it into a nano-dispersion liquid, and ultrasonic vibration is performed for 30 minutes, so that the carbon nanotube particles can be stirred evenly without agglomeration.
[0023] 4) The present invention is applicable to the construction of geopolymer concrete in the field of highway transportation.
[0024] 5) The present invention uses 5-20 mm continuously graded crushed stones to enhance the compactness of geopolymer concrete.
[0025] Table 5 Mix ratio of a reinforced geopolymer concrete containing carbon nanotubes (Kg / m 3 )
[0026] Group Mineral powder Fly ash gravel Sand NaOH Water Glass Carbon Nanotubes water Water-cement ratio 1 262.9 394.3 910.2 390.09 24.24 165 0 395.5 0.35 2 262.9 394.3 910.2 390.09 24.24 165 0.33 395.5 0.35 3 262.9 394.3 910.2 390.09 24.24 165 0.66 395.5 0.35 4 262.9 394.3 910.2 390.09 24.24 165 0.98 395.5 0.35 BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The multi-walled carbon nanotube solution of an embodiment of the present invention;
[0028] Figure 2 This is the carbon nanotube geopolymer concrete after demolding of Example 1. DETAILED DESCRIPTION
[0029] The reinforced geopolymer concrete containing carbon nanotubes of the present invention is prepared by mixing mineral powder, fly ash, crushed stone, sand, carbon nanotubes and a solution of sodium hydroxide and water glass in a certain proportion, and the preparation method thereof comprises:
[0030] (1) According to the designed mix ratio, weigh the following materials by weight, including mineral powder 262.9 kg / m 3 ; Fly ash 394.3Kg / m 3 ;Sand 390.09Kg / m 3 ; Crushed stone 910.2Kg / m 3 ; Water glass 165Kg / m 3 ; Sodium hydroxide 24.24Kg / m3 ; Water 395.5Kg / m 3 ; Carbon nanotube doping 0-0.98Kg / m 3 , water-binder ratio is 0.35;
[0031] (2) further pouring the solid raw materials in (1) into a mixer in order and stirring for 90 seconds to obtain an initial mixture;
[0032] (3) Before the carbon nanotube powder is poured into the blender, 200 ml of water is added to stir it into a nano-dispersion liquid, and ultrasonic vibration is performed for 30 minutes. The remaining water is mixed with weighed NaOH and water glass to form an alkaline excitation solution.
[0033] (4) further pouring the weighed solution into a mixer and stirring for 120 seconds to obtain a final geopolymer concrete mixture;
[0034] (5) further pouring the geopolymer concrete mixture into a triple mold of 100 mm×100 mm×100 mm;
[0035] (6) Further, the mold filled with concrete is placed on a vibration table and vibrated for 60 seconds to make it dense;
[0036] (7) The specimens were further cured at room temperature for 24 hours and then demolded. The molded specimens were placed in a standard curing box with a temperature of 20°C ± 2°C and a humidity of ≥ 95% for curing. After curing for 28 days, a reinforced geopolymer concrete doped with carbon nanotubes was obtained.
[0037] Example 1: This example provides a specific mix ratio of a reinforced geopolymer concrete containing carbon nanotubes:
[0038] Mineral powder Fly ash gravel Sand NaOH Water Glass Carbon Nanotubes water Water-cement ratio 262.9 394.3 910.2 390.09 24.24 165 0 395.5 0.35
[0039] Example 1: This example provides a specific mix ratio of a reinforced geopolymer concrete containing carbon nanotubes:
[0040] Mineral powder Fly ash gravel Sand NaOH Water Glass Carbon Nanotubes water Water-cement ratio 262.9 394.3 910.2 390.09 24.24 165 0.33 395.5 0.35
[0041] Example 1: This example provides a specific mix ratio of a reinforced geopolymer concrete containing carbon nanotubes:
[0042] Mineral powder Fly ash gravel Sand NaOH Water Glass Carbon Nanotubes water Water-cement ratio 262.9 394.3 910.2 390.09 24.24 165 0.66 395.5 0.35
[0043] Example 1: This example provides a specific mix ratio of a reinforced geopolymer concrete containing carbon nanotubes:
[0044] Mineral powder Fly ash gravel Sand NaOH Water Glass Carbon Nanotubes water Water-cement ratio 262.9 394.3 910.2 390.09 24.24 165 0.98 395.5 0.35
[0045] The present invention has the following advantages:
[0046] 1) In the present invention, a large amount of fly ash is added to prepare geopolymer concrete, which can realize the resource utilization of industrial waste, reduce the impact on natural resources, reduce production costs, and meet the requirements of sustainable development.
[0047] 2) The incorporation of an appropriate amount of carbon nanotubes in the present invention can improve the mechanical properties, make it have higher toughness, significantly increase its compressive and tensile strength, and significantly reduce the number and length of cracks.
[0048] 3) The present invention is applicable to the construction of geopolymer concrete in the field of highway transportation.
[0049] 4) The present invention uses 5-20 mm continuously graded crushed stones to enhance the compactness of geopolymer concrete.
Claims
1. A geopolymer concrete mix ratio and preparation method for carbon nanotube-enhanced concrete mechanical properties; characterized in that: The materials of this geopolymer concrete include: mineral powder 262.9Kg / m 3 ; Fly ash 394.3Kg / m 3 ;Sand 390.09Kg / m 3 ; Crushed stone 910.2Kg / m 3 ; Water glass 165Kg / m 3 ; Sodium hydroxide 24.24Kg / m 3 ; Water 395.5Kg / m 3 ; Carbon nanotube doping 0-0.98Kg / m 3 , the water-to-cement ratio is 0.
35.
2. A geopolymer concrete mix ratio and preparation method for carbon nanotube-enhanced concrete mechanical properties according to claim 1; characterized in that The geopolymer is composed of 60% fly ash and 40% mineral powder. The gradation of the coarse aggregate is 5mm-20mm and the density is 2250Kg / m 3 , which is the first-grade fly ash.
3. A geopolymer concrete mix ratio and preparation method for carbon nanotube-enhanced concrete mechanical properties according to claim 1; characterized in that The modulus of the alkali-activated solution is 1.
4.
4. A geopolymer concrete mix ratio and preparation method for carbon nanotube-enhanced concrete mechanical properties according to claim 1; characterized in that The following steps are involved: Step 1: weigh the solid raw materials and liquid raw materials in claim 1 according to the mix ratio of the experimental design; Step 2: further pouring the solid raw materials in claim 1 into a mixer in order and stirring for 90 seconds to obtain an initial mixture; Step 3: Before the carbon nanotube powder is poured into the blender, 200 ml of water is added to stir it into a nano-dispersion liquid, and ultrasonic vibration is performed for 30 minutes. The remaining water is mixed with weighed NaOH and water glass to form an alkaline excitation solution; Step 4: further pouring the weighed solution into a mixer and stirring for 120 seconds to obtain a final geopolymer concrete mixture; Step 5: further pouring the geopolymer concrete mixture into a triple mold of 100 mm×100 mm×100 mm; Step 6: Further place the mold filled with concrete on a vibration table and vibrate for 60 seconds to make it dense; Step 7: The specimens are further cured at room temperature for 24 hours and then demolded. The molded specimens are placed in a standard curing box with a temperature of 20°C ± 2°C and a humidity of ≥ 95% for curing. After curing for 28 days, a reinforced geopolymer concrete doped with carbon nanotubes is obtained.
Citation Information
Cited By
Intelligent sensing geopolymer concrete sensor and preparation method and application thereof
CN122301503A