Method for preparing low-carbon olefin by using light hydrocarbon raw material

By using a combination of core-shell structure dehydrogenation catalyst and molecular sieve catalyst, the yields of ethylene and propylene in catalytic cracking of low-carbon alkanes are improved, the problems of low yield and high energy consumption in the prior art are solved, and efficient catalysis is achieved Lysis reaction.

CN119080577APending Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310640092.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing low-carbon alkane catalytic cracking method still needs to be improved when producing ethylene and propylene, and there are problems of large energy consumption and poor distribution in the production area.

Method used

The dehydrogenation catalyst and molecular sieve catalyst with core-shell structure are used to improve the conversion rate of light hydrocarbon raw materials and the yield of ethylene and propylene through dehydrogenation reaction and catalytic cracking reaction. The specific steps include: using a core-shell structure composed of perovskite manganate and tungstate as a dehydrogenation catalyst, and combining it with a molecular sieve to carry out dehydrogenation and catalytic cracking reactions.

Benefits of technology

The yields of ethylene and propylene are significantly improved, the efficiency of catalytic cracking and product selectivity are improved, and energy consumption is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080577A_ABST
    Figure CN119080577A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing low-carbon olefin by using a light hydrocarbon raw material, which comprises the following steps: (1) contacting the light hydrocarbon raw material with a dehydrogenation catalyst in a dehydrogenation reactor and carrying out dehydrogenation reaction to obtain a dehydrogenation product and hydrogen; and (2) contacting the dehydrogenation product with a cracking catalyst in a catalytic cracking reactor for cracking reaction to obtain a cracking product. According to the technical scheme, the light hydrocarbon raw material rich in alkane and cycloalkane is firstly selectively dehydrogenated to prepare the dehydrogenation product, and then the dehydrogenation product is subjected to the catalytic cracking reaction to generate ethylene and propylene, so that the yield of ethylene and propylene prepared by catalytic cracking of low-carbon alkane is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of petrochemical industry, and in particular to a method for preparing low-carbon olefins by using light hydrocarbon raw materials. Background Art

[0002] Low-carbon olefins such as ethylene and propylene are important basic raw materials for petrochemicals. Driven by downstream demand in recent years, market demand has maintained rapid growth. At present, the production of ethylene and propylene mainly adopts steam thermal cracking. Although this technology has been widely used, it has disadvantages such as high energy consumption and poor distribution of production areas. If catalytic cracking is adopted, the reaction temperature can be lowered, the selectivity of propylene can be improved, and the energy consumption and dry gas generation can be reduced.

[0003] For example, patent document CN102746081B discloses a method for catalytic cracking of a light hydrocarbon mixture obtained by dehydrogenating a raw material containing alkanes and cycloalkanes using a moving bed or fluidized bed reactor, wherein the catalyst needs to be pre-reduced with hydrogen before the reaction, and then reacted and regenerated continuously. The catalyst used in the document is a Pt-Sn / Al2O3 catalyst.

[0004] However, the yields of ethylene and propylene in the existing methods for preparing light olefins by catalytic cracking of light alkanes still need to be further improved. Summary of the invention

[0005] The purpose of the present invention is to improve the yield of ethylene and propylene when preparing light olefins by catalytic cracking of light alkanes.

[0006] In order to achieve the above-mentioned object, the present invention provides a method for preparing low-carbon olefins using light hydrocarbon feedstock, the method comprising: (1) contacting the light hydrocarbon feedstock with a dehydrogenation catalyst in a dehydrogenation reactor and performing a dehydrogenation reaction to obtain a dehydrogenation product and hydrogen; (2) contacting the dehydrogenation product with a cracking catalyst in a catalytic cracking reactor to perform a cracking reaction to obtain a cracking product.

[0007] Optionally, the dehydrogenation catalyst has a core-shell structure, the core of the core-shell structure is perovskite-type manganese salt, and the shell of the core-shell structure is tungstate; the diameter of the core is 10 to 100 nm, and the thickness of the shell is 5 to 100 nm.

[0008] Optionally, the weight ratio of the perovskite-type manganate to the tungstate is 1:(0.1-10), preferably 1:(0.2-6).

[0009] Optionally, the perovskite manganate also contains non-manganese metal elements, and the molar ratio of the manganese element in the perovskite manganate to the non-manganese metal element is 1:(0.1-2), preferably 1:(0.5-1.5); the non-manganese metal element is selected from at least one of Ca, La, Sr, Ba, Ce, Li and Fe.

[0010] Optionally, the dehydrogenation catalyst is prepared by a method comprising the following steps: S1, mixing an aqueous solution of a nitrate containing a non-manganese metal element and manganese nitrate with citric acid and ethylene glycol to obtain a gel, and subjecting the gel to a first drying, roasting and a first calcination to obtain a perovskite-type manganate; S2, impregnating the perovskite-type manganate with an aqueous solution of a soluble tungstate, and then subjecting the perovskite-type manganate to a second drying and a second calcination.

[0011] Optionally, the molar ratio of manganese nitrate to citric acid and ethylene glycol is 1:(1-5):(0.5-7.5); the temperature of the first drying is 100-140°C, and the time is 6-12h; the temperature of the roasting is 300-600°C, and the time is 1-5h; the temperature of the first calcination is 700-1200°C, and the time is 8-12h; the temperature of the second drying is 60-90°C, and the time is 8-10h; the temperature of the second calcination is 700-1000°C, and the time is 6-10h.

[0012] Optionally, the cracking catalyst contains a molecular sieve; the specific surface area of ​​the molecular sieve is 150 to 300 m 2 / g, a silicon-aluminum ratio of 5 to 60, and a pore size of 0.2-5nm; the molecular sieve includes at least one of ZSM-5 molecular sieve, ZSM-11 molecular sieve, β molecular sieve, SAPO-34 molecular sieve and Y molecular sieve.

[0013] Optionally, the final distillation point of the light hydrocarbon feedstock is any value between 20-350° C.; the total content of saturated paraffins and cycloalkanes in the light hydrocarbon feedstock is 30-100 wt %.

[0014] Optionally, the dehydrogenation reactor is a fixed bed reactor, the reaction temperature is 300-750°C, preferably 450-600°C; the weight space velocity is 1-50 (g / hour) / g catalyst, preferably 5-30 (g / hour) / g catalyst.

[0015] Optionally, the cracking reactor is a fixed bed reactor, the reaction temperature is 500-750°C, preferably 600-720°C; the weight space velocity is 1-50 (g / hour) / g catalyst, preferably 5-30 (g / hour) / g catalyst.

[0016] Through the above technical scheme, the present invention first selectively dehydrogenates light hydrocarbon feedstock rich in alkanes and cycloalkanes to obtain dehydrogenated products, and then catalytically cracks the dehydrogenated products to generate ethylene and propylene, thereby further improving the yield of catalytic cracking of low-carbon alkanes to produce ethylene and propylene.

[0017] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0019] Figure 1 This is a scanning electron microscope image of the dehydrogenation catalyst K2WO4 / CaMnO3 of the present invention;

[0020] Figure 2 This is a transmission electron microscope energy spectrum of the dehydrogenation catalyst K2WO4 / CaMnO3 of the present invention. DETAILED DESCRIPTION

[0021] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0022] The present invention provides a method for preparing low-carbon olefins using light hydrocarbon raw materials, the method comprising: (1) contacting the light hydrocarbon raw materials with a dehydrogenation catalyst in a dehydrogenation reactor and performing a dehydrogenation reaction to obtain a dehydrogenation product and hydrogen; (2) contacting the dehydrogenation product with a cracking catalyst in a catalytic cracking reactor to perform a cracking reaction to obtain a cracking product. The method has the advantages of high light hydrocarbon conversion rate and high ethylene and propylene yield.

[0023] According to the present invention, optionally, the dehydrogenation catalyst has a core-shell structure, the core of the core-shell structure is a perovskite-type manganate, and the shell of the core-shell structure is a tungstate; the diameter of the core is 10 to 100 nm, and the thickness of the shell is 5 to 100 nm. The dehydrogenation catalyst of the present invention has a core-shell structure, and when in contact with a light hydrocarbon feedstock, it has high dehydrogenation activity, high selectivity, and good stability.

[0024] According to the present invention, optionally, the weight ratio of the perovskite-type manganate to the tungstate may be 1:(0.1-10), preferably 1:(0.2-6).

[0025] According to the present invention, optionally, the perovskite manganate further contains non-manganese metal elements, and the molar ratio of manganese element in the perovskite manganate to the non-manganese metal elements is 1:(0.1-2), preferably 1:(0.5-1.5).

[0026] According to the present invention, optionally, the non-manganese metal element is selected from at least one of Ca, La, Sr, Ba, Ce, Li and Fe.

[0027] In an embodiment in which the weight ratio of the perovskite manganate to the tungstate is preferably 1:(0.2-6), the molar ratio of the manganese element in the perovskite manganate to the non-manganese metal element is 1:(0.5-1.5), and the non-manganese metal element is La, a dehydrogenation catalyst with excellent performance can be obtained, which can further improve the yield of ethylene and propylene.

[0028] According to the present invention, optionally, the dehydrogenation catalyst may be subjected to reduction pretreatment before the dehydrogenation reaction, the reducing gas is hydrogen, and the reducing temperature is 300-500°C.

[0029] According to the present invention, optionally, the dehydrogenation catalyst is prepared by a method comprising the following steps: S1, mixing an aqueous solution of a nitrate containing a non-manganese metal element and manganese nitrate with citric acid and ethylene glycol to obtain a gel, and subjecting the gel to a first drying, roasting and a first calcination to obtain a perovskite-type manganate; S2, impregnating the perovskite-type manganate with an aqueous solution of a soluble tungstate, and then subjecting the perovskite-type manganate to a second drying and a second calcination.

[0030] According to the present invention, optionally, the molar ratio of manganese nitrate to citric acid and ethylene glycol is 1:(1-5):(0.5-7.5).

[0031] According to the present invention, optionally, the first drying is performed at a temperature of 100-140° C. and for a time of 6-12 hours.

[0032] According to the present invention, optionally, the calcination temperature is 300-600° C. and the calcination time is 1-5 h.

[0033] According to the present invention, optionally, the temperature of the first calcination is 700-1200° C., and the time is 8-12 hours.

[0034] According to the present invention, optionally, the second drying is carried out at a temperature of 60-90° C. and for a time of 8-10 h.

[0035] According to the present invention, optionally, the temperature of the second calcination is 700-1000° C., and the time is 6-10 h.

[0036] According to the present invention, optionally, the cracking catalyst contains a molecular sieve; the specific surface area of ​​the molecular sieve is 150 to 300 m 2 / g, a silicon-aluminum ratio of 5 to 60, and a pore size of 0.2-5nm; the molecular sieve includes at least one of ZSM-5 molecular sieve, ZSM-11 molecular sieve, β molecular sieve, SAPO-34 molecular sieve and Y molecular sieve. The carrier of the cracking catalyst of the present invention includes kaolin, aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, thoria, beryllium oxide, preferably kaolin, aluminum oxide, silicon oxide. During the preparation of the catalyst, phosphoric acid and at least one metal salt of Groups IA, IIA, IB, IIB, IIIB, IVB, and VIIIB of the periodic table can be added to modify the catalyst, preferably phosphoric acid and Fe metal salts.

[0037] According to the present invention, the final boiling point of the light hydrocarbon feedstock is any value between 20-350° C.; the total content of saturated paraffins and cycloparaffins in the light hydrocarbon feedstock is 30-100 wt %.

[0038] According to the present invention, the dehydrogenation reactor is a fixed bed reactor, the reaction temperature is 300-750°C, preferably 450-600°C; the weight space velocity is 1-50 (g / h) / g catalyst, preferably 5-30 (g / h) / g catalyst.

[0039] According to the present invention, the cracking reactor is a fixed bed reactor, the reaction temperature is 500-750°C, preferably 600-720°C; the weight space velocity is 1-50 (g / hour) / g catalyst, preferably 5-30 (g / hour) / g catalyst.

[0040] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0041] The present invention describes the process of preparing a dehydrogenation catalyst and evaluating the catalytic performance of the catalyst using n-octane as a raw material. The dehydrogenation catalyst prepared in the embodiment is evaluated using a fixed bed reactor. A certain amount of catalyst is loaded into a fixed bed reactor, and the dehydrogenation catalyst and the cracking catalyst are placed in two reaction zones, respectively, separated by quartz wool. N-octane is injected by an injection pump to perform a catalytic cracking reaction. The gas product is analyzed online by a gas chromatograph to obtain a detailed composition of the cracked gas.

[0042] The raw material n-octane (mass fraction greater than 99.0%) in the examples is analytically pure and is a product of Acros Organics Reagent Company.

[0043] Example 1

[0044] In this embodiment, the core-shell structure of K2WO4 / CaMnO3 is synthesized according to the following steps: Step a), Mn(NO3)2·4H2O and Ca(NO3)2·4H2O are dissolved in deionized water at a molar ratio of 1:1, and stirred at 40°C for 30 minutes. Add citric acid at a molar ratio of 2.5:1 to metal ions, and stir the solution at 500rpm and 40°C for 30 minutes. Add ethylene glycol at a molar ratio of 1.5:1 to citric acid to promote gel formation, and continue to stir the solution and heat it to 80°C until a sticky gel appears. Then dry at 120°C for 8h, calcine in a muffle furnace at 450°C for 3h to remove nitrates, and calcine in a tubular furnace at 1000°C for 10h with a gas flow rate of 100mL / min to obtain the perovskite core material CaMnO3. Step b), dissolving K2WO4·4H2O in a mass ratio of 1:5 to the perovskite core material CaMnO3 in deionized water, impregnating the perovskite core material, stirring for 1 hour, drying at 80°C for 8 hours, and calcining at 900°C for 8 hours to obtain a core-shell structure dehydrogenation catalyst K2WO4 / CaMnO3. The scanning electron microscope and high-magnification transmission electron microscope energy spectrum of the core-shell structure dehydrogenation catalyst K2WO4 / CaMnO3 are as follows Figure 1 and 2 shown.

[0045] A K2WO4 / CaMnO3 dehydrogenation catalyst with a core-shell structure and a cracking catalyst containing a ZSM-5 molecular sieve are used. The two catalysts are placed in two reaction zones in the reactor respectively and separated by quartz wool in the middle.

[0046] Taking n-octane as raw material, under the conditions of reaction temperature of 600°C, pressure of 0.1MPa and weight space velocity of 12 (g / hour) / g catalyst, the single-pass n-octane conversion rate is 79.02%, and the yields of ethylene, propylene and hydrogen are 12.46%, 20.05% and 4.87% respectively.

[0047] Example 2

[0048] In this embodiment, Na2WO4 / LaMnO3 with a core-shell structure is synthesized: Step a), Mn(NO3)2·4H2O and La(NO3)3·6H2O are dissolved in deionized water at a molar ratio of 1:1 and stirred at 40°C for 30 min. Add citric acid at a molar ratio of 2.5:1 to metal ions, and stir the solution at 500rpm and 40°C for 30 min. Add ethylene glycol at a molar ratio of 1.5:1 to citric acid to promote gel formation, and continue stirring the solution and heat it to 80°C until a sticky gel appears. Then dry at 120°C for 8h, calcine in a muffle furnace at 450°C for 3h to remove nitrates, and calcine in a tubular furnace at 1000°C for 10h with a gas flow rate of 100mL / min to obtain a perovskite core material LaMnO3. Step b), dissolving Na2WO4·4H2O in a mass ratio of 1:5 to the perovskite core material LaMnO3 in deionized water, impregnating the perovskite core material, stirring for 1 hour, drying at 80°C for 8 hours, and calcining at 900°C for 8 hours to obtain a core-shell structure dehydrogenation catalyst Na2WO4 / LaMnO3.

[0049] Na2WO4 / LaMnO3 is used as a dehydrogenation catalyst, and a cracking catalyst containing a ZSM-5 molecular sieve is used. The two catalysts are placed in two reaction zones in the reactor respectively, separated by quartz wool in the middle.

[0050] Taking n-octane as raw material, under the conditions of reaction temperature of 600°C, pressure of 0.1MPa and weight space velocity of 12 (g / hour) / g catalyst, the conversion rate of n-octane in one pass is 85.1%, and the yields of ethylene, propylene and hydrogen are 12.78%, 21.07% and 5.28% respectively.

[0051] Example 3

[0052] The preparation method of the core-shell structured Na2WO4 / SrMnO3 dehydrogenation catalyst in this embodiment is the same as that in Example 2, except that Mn(NO3)2·4H2O and Sr(NO3)3·6H2O are dissolved in deionized water in a molar ratio of 1:1 to obtain the perovskite core material SrMnO3.

[0053] Na2WO4 / SrMnO3 is used as a dehydrogenation catalyst, and a cracking catalyst containing a ZSM-5 molecular sieve is used. The two catalysts are placed in two reaction zones in the reactor respectively, separated by quartz wool in the middle.

[0054] Taking n-octane as raw material, under the conditions of reaction temperature of 600°C, pressure of 0.1MPa and weight space velocity of 12 (g / hour) / g catalyst, the single-pass n-octane conversion rate is 77.3%, and the yields of ethylene, propylene and hydrogen are 11.62%, 19.24% and 4.69% respectively.

[0055] Comparative Example 1

[0056] When K2WO4 / CaMnO3 prepared in Example 1 is used alone as a dehydrogenation catalyst, with n-octane as a raw material, under the conditions of a reaction temperature of 600°C, a pressure of 0.1 MPa, and a weight space velocity of 12 (g / hour) / g catalyst, the single-pass n-octane conversion rate is 5.82%, and the yields of ethylene, propylene and hydrogen are 0.64%, 0.47% and 0.29% respectively.

[0057] Comparative Example 2

[0058] When a cracking catalyst containing ZSM-5 molecular sieve is used alone, with n-octane as raw material, at a reaction temperature of 600°C, a pressure of 0.1 MPa, and a weight space velocity of 12 (g / h) / g catalyst, the single-pass n-octane conversion rate is 72.81%, and the yields of ethylene, propylene and hydrogen are 10.94%, 19.3% and 4.42% respectively.

[0059] The properties of the catalyst, reaction conditions and reaction products are shown in Table 1.

[0060] Table 1

[0061]

[0062] As can be seen from Table 1, the method of the present invention can improve the yields of ethylene, propylene and hydrogen. In addition, preferably using Na2WO4 / LaMnO3 as a dehydrogenation catalyst and using a cracking catalyst containing ZSM-5 molecular sieve, when performing a catalytic cracking reaction, the yields of ethylene, propylene and hydrogen can be further improved.

[0063] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0064] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0065] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing low-carbon olefins using light hydrocarbon feedstocks, characterized in that: The method comprises: (1) contacting a light hydrocarbon feedstock with a dehydrogenation catalyst in a dehydrogenation reactor and performing a dehydrogenation reaction to obtain a dehydrogenation product and hydrogen; and (2) contacting the dehydrogenation product with a cracking catalyst in a catalytic cracking reactor and performing a cracking reaction to obtain a cracking product.

2. The method according to claim 1, wherein: The dehydrogenation catalyst has a core-shell structure, the core of the core-shell structure is perovskite-type manganate, and the shell of the core-shell structure is tungstate; the diameter of the core is 10-100nm, and the thickness of the shell is 5-100nm.

3. The method according to claim 1 or 2, wherein: The weight ratio of the perovskite-type manganate to the tungstate is 1:(0.1-10), preferably 1:(0.2-6).

4. The method according to claim 3, wherein: The perovskite-type manganate further contains a non-manganese metal element, and the molar ratio of the manganese element in the perovskite-type manganate to the non-manganese metal element is 1:(0.1-2), preferably 1:(0.5-1.5); The non-manganese metal element is selected from at least one of Ca, La, Sr, Ba, Ce, Li and Fe.

5. The method according to claim 4, wherein: The dehydrogenation catalyst is prepared by a method comprising the following steps: S1, mixing an aqueous solution of a nitrate containing a non-manganese metal element and manganese nitrate with citric acid and ethylene glycol to obtain a gel, and subjecting the gel to a first drying, roasting and first calcining to obtain a perovskite-type manganate; S2, impregnating the perovskite-type manganate with an aqueous solution of soluble tungstate, and then performing a second drying and a second calcination.

6. The method according to claim 5, wherein: The molar ratio of manganese nitrate to citric acid and ethylene glycol is 1:(1-5):(0.5-7.5); The first drying temperature is 100-140°C and the time is 6-12h; The calcination temperature is 300-600°C and the calcination time is 1-5h; The first calcination temperature is 700-1200°C and the time is 8-12h; The second drying temperature is 60-90°C and the time is 8-10h; The second calcination is carried out at a temperature of 700-1000° C. and for a time of 6-10 hours.

7. The method according to claim 1, wherein: The cracking catalyst contains a molecular sieve; the specific surface area of ​​the molecular sieve is 150 to 300 m 2 / g, a silicon-aluminum ratio of 5 to 60, and a pore size of 0.2-5nm; the molecular sieve includes at least one of ZSM-5 molecular sieve, ZSM-11 molecular sieve, β molecular sieve, SAPO-34 molecular sieve and Y molecular sieve.

8. The method according to claim 1, wherein: The final boiling point of the light hydrocarbon feedstock is any value between 20°C and 350°C; the total content of saturated paraffins and cycloparaffins in the light hydrocarbon feedstock is 30 to 100 wt%.

9. The method according to claim 1, wherein: The dehydrogenation reactor is a fixed bed reactor, the reaction temperature is 300-750°C, preferably 450-600°C; the weight space velocity is 1-50 (g / hour) / g catalyst, preferably 5-30 (g / hour) / g catalyst.

10. The method according to claim 1, wherein: The cracking reactor is a fixed bed reactor, the reaction temperature is 500-750°C, preferably 600-720°C; the weight space velocity is 1-50 (g / hour) / g catalyst, preferably 5-30 (g / hour) / g catalyst.