Tetrahydronaphthol-phosphine pre-transition metal complex as well as preparation method and application thereof

By maintaining high activity in olefin polymerization catalysis by tetrahydronaphthol-phosphine transition metal complex, the problem of decreasing activity of catalysts at high temperatures in the prior art is solved, and the molecular weight and performance of the polymer are improved.

CN119080830APending Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310659028.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing olefin polymerization catalysts cannot maintain high catalytic activity and high polymerization performance at high temperatures, which limits the development of high-end polyolefin production.

Method used

Develop a tetrahydronaphthol-phosphine transition metal complex that maintains high ethylene polymerization activity at higher temperatures and is used for olefin polymerization catalysis, including main catalysts, by specific preparation methods and applications. and a cocatalyst.

Benefits of technology

实现了在高温条件下保持高催化活性和聚合性能,制备的聚合物分子量分布较窄,提高了烯烃聚合物的性能。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080830A_ABST
    Figure CN119080830A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of olefin polymerization catalysts, and discloses a tetrahydronaphthol-phosphine pre-transition metal complex as well as a preparation method and application thereof. The structural formula of the tetrahydronaphthol-phosphine pre-transition metal complex is shown as a formula (I), and M is selected from IVB group metal; ar is selected from substituted or unsubstituted C6-C20 aryl groups; x is selected from halogen or C1-C10 alkyl, and n is 1 or 2. When the tetrahydronaphthol-phosphorus pre-transition metal complex is used as a main catalyst, the tetrahydronaphthol-phosphorus pre-transition metal complex has higher homopolymerization / copolymerization activity under similar polymerization conditions, and an obtained polymer is higher in molecular weight and narrower in distribution. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of olefin polymerization catalysts, and in particular to a tetralinol-phosphine pre-transition metal complex and a preparation method and application thereof. Background Art

[0002] Polyethylene materials have the characteristics of good chemical resistance, low price, simple preparation, low density, good mechanical properties, etc., and can also be used as a potential rubber substitute. In addition, by introducing polar functional groups into polyolefins composed of saturated carbon chains, the application performance of the materials can be greatly improved and the development direction of the materials can be expanded. Therefore, it is urgent to develop high value-added and high-performance polyolefin products.

[0003] Metal complexes are currently the most commonly used olefin polymerization catalysts, mainly including homogeneous and heterogeneous catalysts. Among the many types of olefin polymerization catalysts, homogeneous pre-transition metal catalysts have high polymerization activity, high molecular weight of the resulting polymer, can achieve active polymerization, and have many advantages such as controllability, so they have attracted much attention from scholars (see, for example, Angew. Chem. Int. Ed. 2020, 59, 14726–147; Chemical Bulletin, 2014, 77, 951–960). By changing the steric hindrance effect, electronic effect and number of metal centers near the active center, the purpose of regulating polymerization activity, polymerization products and product distribution can be achieved. However, my country is relatively backward in the production of high-end polyolefins. Among them, the lack of olefin polymerization catalysts with good performance is the main factor restricting the development of this field. At present, the existing ethylene gas phase polymerization process usually requires a polymerization temperature of more than 85°C, and the ethylene solution polymerization process usually requires a polymerization temperature of 130-250°C. However, the existing olefin polymerization catalysts all have the problem of being unable to maintain high catalytic activity and high polymerization performance at high temperatures. Summary of the invention

[0004] The object of the present invention is to provide a tetrahydronaphthol-phosphine transition metal complex and a preparation method and application thereof, wherein the tetrahydronaphthol-phosphine transition metal complex has good thermal stability. In particular, the tetrahydronaphthol-phosphine transition metal complex can still maintain a high ethylene polymerization activity at a relatively high temperature, and the molecular weight distribution of the obtained polymer is relatively narrow.

[0005] In order to achieve the above object, the present invention provides a tetrahydronaphthol-phosphine transition metal complex, the structural formula of which is shown in formula (I):

[0006]

[0007] Wherein, M is selected from Group IVB metals; Ar is selected from substituted or unsubstituted C6-C20 aromatic groups; X is selected from halogen or C1-C10 hydrocarbon groups, and n is 1 or 2.

[0008] Preferably, the structural formula of the tetrahydronaphthol-phosphine transition metal complex is as shown in formula (II),

[0009]

[0010] Among them, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C20 hydrocarbon groups.

[0011] Preferably, M is selected from Ti, Zr or Hf.

[0012] Preferably, X is selected from halogen or C1-C8 hydrocarbon group, and n is 1 or 2.

[0013] Preferably, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxy, substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C15 aryl.

[0014] Preferably, the substituents are selected from halogen, hydroxy, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy.

[0015] Preferably, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl.

[0016] Preferably, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy.

[0017] Preferably, the halogen is selected from fluorine, chlorine, bromine or iodine.

[0018] The second aspect of the present invention provides a method for preparing the above-mentioned tetrahydronaphthol-phosphine transition metal complex, the method comprising:

[0019] (1) reacting the compound represented by formula (III) with the compound represented by formula (IV) to generate a ligand;

[0020] (2) reacting the ligand with a second hydrogen extraction agent, and then reacting with an M metal compound;

[0021]

[0022] Wherein, the metal M in the M metal compound is selected from Group IVB metals, and the definition of Ar is the same as described above.

[0023] Preferably, the M metal compound is selected from one or more of titanium tetrachloride, bis(tetrahydrofuran)titanium tetrachloride, tris(tetrahydrofuran)titanium trichloride, zirconium tetrachloride, bis(tetrahydrofuran)zirconium tetrachloride, hafnium tetrachloride, and bis(tetrahydrofuran)hafnium tetrachloride.

[0024] Preferably, the second hydrogen abstraction agent is selected from one or more of NaH, KH, n-butyllithium, and methyllithium.

[0025] The third aspect of the present invention provides the application of the above tetrahydronaphthol-phosphine early transition metal complex in olefin polymerization.

[0026] The fourth aspect of the present invention provides a catalyst for olefin polymerization, and the catalyst for olefin polymerization includes a main catalyst and a cocatalyst;

[0027] The main catalyst is the above tetrahydronaphthol-phosphine early transition metal complex.

[0028] Preferably, the cocatalyst is an organoaluminum compound and / or an organoboron compound.

[0029] Preferably, the organoaluminum compound is selected from alkylaluminoxane or an organoaluminum compound of the general formula AlY n Z 3-n wherein Y is selected from hydrogen, a C1-C20 hydrocarbon group, or a C1-C20 hydrocarbyloxy group, Z is selected from a halogen, 0 < n ≤ 3, and n is an integer.

[0030] Preferably, Y is selected from a C1-C20 alkyl group, a C1-C20 alkoxy group, a C7-C20 aralkyl group, or a C6-C20 aryl group.

[0031] Preferably, Z is selected from chlorine or bromine.

[0032] Preferably, the organoboron compound is selected from arylboron and / or organoborate.

[0033] The fifth aspect of the present invention provides the application of the above catalyst for olefin polymerization in olefin polymerization.

[0034] The sixth aspect of the present invention provides an olefin polymerization method, including performing an olefin polymerization reaction in the presence of the above catalyst for olefin polymerization.

[0035] Preferably, the temperature of the polymerization reaction is -78°C to 200°C, more preferably -20°C to 150°C; the polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.

[0036] When the tetrahydronaphthol-phosphine transition metal complex of the present invention is used as a main catalyst in olefin polymerization, it has high homopolymerization / copolymerization activity, can catalyze olefin polymerization at a higher temperature, and the prepared olefin polymer has a significantly higher molecular weight.

[0037] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0038] (1) The synthesis method of the tetrahydronaphthol-phosphine transition metal complex of the present invention is simple and easy;

[0039] (2) The tetrahydronaphthol-phosphine transition metal complex of the present invention can catalyze ethylene polymerization with high activity, and in particular, can maintain high polymerization activity at a relatively high polymerization temperature;

[0040] (3) The olefin polymerization catalyst of the present invention has higher performance in copolymerization of ethylene with α-olefins or polar monomers. DETAILED DESCRIPTION

[0041] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0042] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0043] In one aspect, the present invention provides a tetralinol-phosphine transition metal complex, the structural formula of which is shown in formula (I):

[0044]

[0045] Wherein, M is selected from Group IVB metals; Ar is selected from substituted or unsubstituted C6-C20 aromatic groups; X is selected from halogen or C1-C10 hydrocarbon groups, and n is 1 or 2.

[0046] Preferably, Ar is a substituted or unsubstituted C6-C15 aryl group.

[0047] According to some embodiments of the invention, Ar is a substituted or unsubstituted C6-C8 aryl group.

[0048] In a preferred embodiment, the structural formula of the tetrahydronaphthol-phosphine transition metal complex is as shown in formula (II),

[0049]

[0050] Among them, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C20 hydrocarbon groups.

[0051] In a preferred embodiment, M is selected from Ti, Zr or Hf.

[0052] In a preferred embodiment, X is selected from halogen or C1-C8 hydrocarbon group (such as C1-C6 alkyl group).

[0053] In a more preferred embodiment, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxy, substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C15 aryl.

[0054] In the present invention, n is 1 or 2, and n represents the number of X groups connected to the metal M.

[0055] In the present invention, the "substituted" in "substituted or unsubstituted" refers to containing substituents, and the substituents here can be selected from halogen, hydroxyl, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy.

[0056] In the present invention, the alkyl group (such as C1-C6 alkyl group, C1-C10 alkyl group) can be selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl.

[0057] In the present invention, the alkoxy group (such as C1-C6 alkoxy group) can be selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy.

[0058] In the present invention, the aryl group (such as a C6-C10 aryl group or a C6-C15 aryl group) may be selected from a phenyl group, a 4-methylphenyl group, a 4-ethylphenyl group, a dimethylphenyl group or a vinylphenyl group.

[0059] In the present invention, the halogen is selected from fluorine, chlorine, bromine or iodine.

[0060] In a further preferred embodiment, the tetrahydronaphthol-phosphine transition metal complex is selected from the group consisting of the following complexes:

[0061] Complex 1: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=1;

[0062] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0063] Complex 3: A complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is methyl, n=2;

[0064] Complex 4: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is -CH2C6H5, n=2;

[0065] Complex 5: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is Cl, and n=1;

[0066] Complex 6: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is Cl, n=2;

[0067] Complex 7: A complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2;

[0068] Complex 8: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2;

[0069] Complex 9: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=1;

[0070] Complex 10: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2;

[0071] Complex 11: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2;

[0072] Complex 12: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2;

[0073] Complex 13: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=1;

[0074] Complex 14: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2;

[0075] Complex 15: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2;

[0076] Complex 16: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2;

[0077] Complex 17: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=1;

[0078] Complex 18: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2;

[0079] Complex 19: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2;

[0080] Complex 20: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, n=2;

[0081] Complex 21: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is Cl, n=2;

[0082] Complex 22: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is methyl, n=2;

[0083] Complex 23: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is -CH2C6H5, n=2;

[0084] Complex 24: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is Cl, n=2;

[0085] Complex 25: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2;

[0086] Complex 26: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2;

[0087] Complex 27: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2;

[0088] Complex 28: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2;

[0089] Complex 29: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2;

[0090] Complex 30: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2;

[0091] Complex 31: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2;

[0092] Complex 32: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2;

[0093] Complex 33: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2;

[0094] Complex 34: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2;

[0095] Complex 35: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, n=2;

[0096] Complex 36: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is Cl, n=2;

[0097] Complex 37: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is methyl, n=2;

[0098] Complex 38: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is -CH2C6H5, n=2;

[0099] Complex 39: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is Cl, n=2;

[0100] Complex 40: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2;

[0101] Complex 41: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2;

[0102] Complex 42: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2;

[0103] Complex 43: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2;

[0104] Complex 44: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2;

[0105] Complex 45: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2;

[0106] Complex 46: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2;

[0107] Complex 47: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2;

[0108] Complex 48: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2;

[0109] Complex 49: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2;

[0110] Complex 50: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, and n=2.

[0111] The second aspect of the present invention provides a method for preparing the above-mentioned tetrahydronaphthol-phosphine transition metal complex, the method comprising:

[0112] (1) reacting the compound represented by formula (III) with the compound represented by formula (IV) to generate a ligand;

[0113] (2) reacting the ligand with a second hydrogen extraction agent, and then reacting with an M metal compound;

[0114]

[0115] Wherein, the metal M in the M metal compound is selected from Group IVB metals, and the definition of Ar is the same as described above.

[0116] In the method described in the present invention, the specific reaction process is shown in the following reaction formula.

[0117]

[0118] wherein Ar, M, X and n are as defined above.

[0119] In a more preferred embodiment, the reaction process of step (1) is shown in the following reaction formula.

[0120]

[0121] Among them, R7-R 11 The definition of is the same as described above.

[0122] In a more preferred embodiment, the reaction process of step (2) is shown in the following reaction formula.

[0123]

[0124] Among them, R7-R 11 The definitions of M, X and n are the same as described above.

[0125] In the method of the present invention, preferably, the metal M in the M metal compound is selected from Ti, Zr or Hf.

[0126] In a preferred embodiment, the M metal compound is selected from one or more of titanium tetrachloride, bis(tetrahydrofuran)titanium tetrachloride (TiCl4(THF)2), tris(tetrahydrofuran)titanium trichloride, zirconium tetrachloride, bis(tetrahydrofuran)zirconium tetrachloride ((THF)2ZrCl4), hafnium tetrachloride and bis(tetrahydrofuran)hafnium tetrachloride ((THF)2HfCl4).

[0127] In the present invention, "THF" means "tetrahydrofuran".

[0128] In a preferred embodiment, during the reaction of step (1), the compound represented by formula (III) is first reacted with a first hydrogen extraction agent and then reacted with the compound represented by formula (IV).

[0129] In the method of the present invention, the reaction of step (2) is carried out in the presence of a reaction solvent.

[0130] According to some embodiments of the present invention, the reaction solvent may be toluene or tetrahydrofuran.

[0131] In a specific embodiment, the reaction solvent is tetrahydrofuran.

[0132] In the method of the present invention, the first hydrogen withdrawal agent used in step (1) and the second hydrogen withdrawal agent used in step (2) may be the same or different, and the first hydrogen withdrawal agent and the second hydrogen withdrawal agent are each independently selected from one or more of NaH, KH, n-butyl lithium and methyl lithium.

[0133] In a specific embodiment, the preparation process of step (1) comprises: in a protective gas (such as nitrogen) atmosphere, dissolving the compound represented by formula (III) in anhydrous ether in a nitrogen atmosphere, adding a first hydrogen extraction agent solution (such as n-butyl lithium) dropwise at -78°C, and gradually returning the reaction to room temperature; adding a tetrahydrofuran solution (ice-water bath) of the phosphine compound represented by formula (IV) dropwise to the original reaction system, slowly warming to room temperature, stirring the reaction overnight, quenching with water, extracting the organic phase with ether, concentrating the obtained organic phase, deoxygenating by freezing cycle, adding 5 mL of concentrated hydrochloric acid to react under a nitrogen atmosphere, tracking the reaction completion with TLC, and then adding a NaHCO3 aqueous solution to neutralize, quenching with water, extracting the organic phase with ether, drying with anhydrous MgSO4, filtering, concentrating, and column chromatography to obtain the ligand represented by formula (V).

[0134] In a specific embodiment, the preparation process of step (2) comprises: in a protective gas (such as nitrogen) atmosphere, dissolving the ligand obtained in step (1) in an organic solvent (such as toluene, tetrahydrofuran, etc.), adding an excess of a second hydrogen extraction agent (such as NaH, KH, etc.), stirring at room temperature, filtering to remove the hydrogen extraction agent, and then dissolving the M metal compound in an organic solvent (such as toluene, tetrahydrofuran, etc.), and adding dropwise to the original reaction system, reacting overnight, draining the solvent, adding dichloromethane to dissolve, filtering to remove the filter cake, concentrating the filtrate, and adding heptane for recrystallization to obtain the tetrahydronaphthol-phosphine pre-transition metal complex of the present invention.

[0135] The third aspect of the present invention provides the use of the above tetrahydronaphthol-phosphine early transition metal complex in olefin polymerization.

[0136] Preferably, the olefins include ethylene, α-olefins containing polar groups and cyclic olefins.

[0137] A fourth aspect of the present invention provides a catalyst for olefin polymerization, wherein the catalyst for olefin polymerization comprises a main catalyst and a co-catalyst;

[0138] The main catalyst is the above-mentioned tetralin-phosphine pre-transition metal complex.

[0139] In the present invention, the co-catalyst may be selected from organoaluminum compounds and / or organoboron compounds.

[0140] In a preferred embodiment, the organoaluminum compound is selected from alkylaluminoxanes or organoaluminum compounds having the general formula AlY n Z 3-n , wherein Y is selected from hydrogen, C1-C20 hydrocarbon groups or C1-C20 alkoxy groups, Z is selected from halogens, 0 < n ≤ 3, and n is an integer.

[0141] In a more preferred embodiment, Y is selected from C1-C20 alkyl groups, C1-C20 alkoxy groups, C7-C20 aralkyl groups or C6-C20 aryl groups.

[0142] According to some embodiments of the present invention, Z is selected from chlorine or bromine.

[0143] Further preferably, the organoaluminum compound is selected from one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, trioctylaluminum, diethylaluminum hydride, diisobutylaluminum hydride, diethylaluminum chloride, diisobutylaluminum chloride, sesquiethylaluminum chloride, dichloroethylaluminum, methylaluminoxane (MAO), and modified methylaluminoxane (MMAO).

[0144] In a specific embodiment, the organoaluminum compound is methylaluminoxane (MAO).

[0145] In a preferred embodiment, the organoboron compound is selected from arylborons and / or organoboronates.

[0146] In a more preferred embodiment, the arylboron is substituted or unsubstituted phenylboron.

[0147] In a specific embodiment, the arylboron is tris(pentafluorophenyl)boron.

[0148] In a more preferred embodiment, the organoborate is N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate and / or triphenylmethyl tetrakis(pentafluorophenyl)borate.

[0149] In a preferred embodiment, when the cocatalyst is an organoaluminum compound, the molar ratio of aluminum in the cocatalyst to metal M in the main catalyst is 10-10 7 :1, preferably 10-100000:1, more preferably 100-10000:1; specifically, the molar ratio can be 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 500:1, 700:1, 800:1, 1000:1, 2000:1, 3000:1, 5000:1, 10000:1, 100000:1, 1000000:1, 10000000:1 or any value therebetween.

[0150] In a preferred embodiment, when the co-catalyst is an organic boron compound, the molar ratio of boron in the co-catalyst to the metal M in the main catalyst is 0.1-1000:1, preferably 0.1-500:1; specifically, the molar ratio can be 0.1:1, 0.2:1, 0.5:1, 1:1, 2:1, 3:1, 5:1, 8:1, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 500:1, 700:1, 800:1, 1000:1 or any value therebetween.

[0151] In the present invention, the olefin is a C2-C16 olefin.

[0152] In a preferred embodiment, the olefin is ethylene or an α-olefin having 3 to 16 carbon atoms.

[0153] A fifth aspect of the present invention provides use of the above-mentioned olefin polymerization catalyst in olefin polymerization.

[0154] Preferably, the olefins include ethylene, α-olefins containing polar groups and cyclic olefins.

[0155] The sixth aspect of the present invention also provides an olefin polymerization method, comprising carrying out an olefin polymerization reaction in the presence of the above-mentioned olefin polymerization catalyst.

[0156] In a preferred embodiment, the polymerization reaction temperature is -78°C to 200°C, more preferably -20°C to 150°C; the polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.

[0157] According to some embodiments of the present invention, the polymerization reaction temperature may be -20°C, 50°C, 100°C or 150°C.

[0158] According to some embodiments of the present invention, the polymerization pressure may be 0.01 MPa, 0.1 MPa, 0.2 MPa, 0.5 MPa, 1 MPa or 2 MPa.

[0159] In a preferred embodiment, the polymerization reaction time is 5 to 60 minutes.

[0160] In a specific embodiment, the polymerization reaction time is 30 min.

[0161] In the present invention, the olefin polymerization reaction may be homopolymerization or copolymerization.

[0162] In the present invention, "polymerization pressure" refers to the ethylene pressure in the polymerization system and is expressed as an absolute pressure.

[0163] In the olefin polymerization method of the present invention, the olefin is a C2-C16 olefin.

[0164] According to one embodiment of the present invention, the olefin comprises ethylene.

[0165] According to one embodiment of the present invention, the olefins include ethylene, propylene, α-olefins, and cycloolefins.

[0166] According to some embodiments of the present invention, the olefin polymerization reaction is carried out by using olefin monomers in a solvent, and the polymerization solvent is selected from one or more of alkanes, aromatic hydrocarbons and halogenated hydrocarbons.

[0167] According to some specific embodiments of the present invention, the polymerization solvent is selected from one or more of hexane, pentane, heptane, benzene, toluene, dichloromethane, chloroform, chlorobenzene and dichloroethane, preferably one or more of hexane, toluene and heptane.

[0168] According to some embodiments of the present invention, the process of catalyzing the homopolymerization of ethylene using a tetralinol-phosphine pre-transition metal complex as the main catalyst for olefin polymerization is as follows: ethylene and the olefin polymerization catalyst are subjected to a high-pressure solution polymerization reaction in an inert solvent, and after the reaction is completed, the polymer is precipitated using a precipitant, and then filtered and dried.

[0169] In a preferred embodiment, the inert solvent is toluene, xylene or decahydronaphthalene; and the precipitant is methanol, ethanol or acetone.

[0170] In a specific embodiment, the inert solvent is toluene.

[0171] In the present invention, the olefin polymerization catalyst using the tetrahydronaphthol-phosphine transition metal complex as the main catalyst has excellent homopolymerization activity and stability of ethylene homopolymerization, which can reach up to 5.6×10 7 g / (mol·h), and can still reach 10 under the polymerization conditions of 80℃ 6 g / (mol·h).

[0172] According to some embodiments of the present invention, the specific reaction process of the direct coordination copolymerization of ethylene and a comonomer (α-olefin and / or cycloolefin containing a polar group) catalyzed by a catalyst for olefin polymerization using a tetralin-phosphine pre-transition metal complex as the main catalyst is as follows: ethylene, the comonomer and the olefin polymerization catalyst are subjected to a solution polymerization reaction in an inert solvent, and after the reaction is completed, the polymer is precipitated using a precipitant, and then filtered and dried.

[0173] In a preferred embodiment, the inert solvent is toluene, xylene or decahydronaphthalene; and the precipitant is methanol, ethanol or acetone.

[0174] In a specific embodiment, the inert solvent is toluene.

[0175] In the present invention, the olefin polymerization catalyst using the tetrahydronaphthol-phosphine transition metal complex as the main catalyst catalyzes the direct coordination copolymerization of ethylene and comonomers (α-olefins and / or cycloolefins containing polar groups) with a maximum activity of 4.1×10 5 g / (mol·h), and the insertion rate of the comonomer and the molecular weight of the copolymer are relatively high.

[0176] In a specific embodiment, the comonomers are long-chain α-olefins and norbornene.

[0177] In a preferred embodiment, the molar ratio of the comonomer to the olefin polymerization catalyst is 0-1000:1; specifically, it can be 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1 or 1000:1.

[0178] In a preferred embodiment, the amount of the olefin polymerization catalyst used is 5-30 μmol; specifically, it can be 5 μmol, 10 μmol, 15 μmol, 20 μmol, 25 μmol or 30 μmol.

[0179] In a preferred embodiment, the polymerization pressure is 0.1-3 MPa, the polymerization reaction temperature is 30-100°C, and the polymerization reaction time is 10-60 min; specifically, the polymerization pressure may be 0.1 MPa, 0.5 MPa, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa or 3 MPa; the polymerization reaction temperature may be 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C; the polymerization reaction time may be 10 min, 20 min, 30 min, 40 min, 50 min or 60 min.

[0180] In the present invention, alkyl refers to a straight chain alkyl, a branched alkyl or a cycloalkyl, including but not limited to: methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, n-decyl, cyclopropyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-ethylcyclohexyl, 4-n-propylcyclohexyl and 4-n-butylcyclohexyl.

[0181] In the present invention, alkenyl refers to straight-chain alkenyl, branched-chain alkenyl or cycloalkenyl, including but not limited to vinyl, allyl and butenyl.

[0182] In the present invention, examples of the aralkyl group include, but are not limited to, phenylmethyl, phenylethyl, phenyl-n-propyl, phenyl-isopropyl, phenyl-n-butyl and phenyl-t-butyl.

[0183] In the present invention, examples of the alkylaryl group include, but are not limited to, tolyl, ethylphenyl, n-propylphenyl, isopropylphenyl, n-butylphenyl and tert-butylphenyl.

[0184] The tetrahydronaphthol-phosphine transition metal complex and its preparation method and application described in the present invention are further illustrated by examples. The embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.

[0185] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0186] The analytical characterization instruments and test methods used in the following examples and comparative examples are as follows:

[0187] (1) Nuclear magnetic resonance instrument: Bruker DMX 300 (300 MHz), with tetramethylsilane (TMS) as internal standard;

[0188] (2) Molecular weight and molecular weight distribution PDI of polymer (PDI = Mw / Mn): measured at 150°C using PL-GPC220 chromatograph with trichlorobenzene as solvent (standard sample: PS, flow rate: 1.0 mL / min, chromatographic column: 3×PLgel 10um M1×ED-B, 300×7.5 nm);

[0189] (3) Activity measurement method: The polymer was washed with hydrochloric acid ethanol solution, vacuum dried, and the weight of the polymer was measured; the polymerization activity was calculated as follows: polymer weight (g) / metal (mol) × 60 / polymerization time (min);

[0190] (4) Analysis of the comonomer content of polymers: 1 H NMR, 13 C NMR spectrum was determined on a 400 MHz Bruker Avance 400 NMR spectrometer using a 10 mm PASEX 13 probe. The polymer sample was dissolved in 1,2,4-trichlorobenzene at 120°C for analysis and testing.

[0191] Example 1

[0192] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0193] In a nitrogen atmosphere, the compound represented by formula (III) (2.32 g, 10 mmol) was dissolved in anhydrous ether (20 mL), and n-butyl lithium solution (2.7 M, 4.0 mL, 11 mmol) was added dropwise at -78 ° C. The reaction was gradually restored to room temperature and stirred for 12 h to obtain a white precipitate. Diphenylphosphine chloride (PPh2Cl) (11 mmol, 2.42 g) was evenly dispersed in 10 mL of ether and added dropwise to the original reaction system under an ice-water bath. The temperature was slowly raised to room temperature and stirred overnight. The mixture was quenched with water, and the organic phase was extracted with ether. The obtained organic phase was concentrated, deoxygenated by freezing cycle, and 5 mL of concentrated hydrochloric acid was added under a nitrogen atmosphere to react for 5 h. The reaction was followed by TLC to complete, and then a NaHCO3 aqueous solution was added for neutralization, quenched with water, and the organic phase was extracted with ether. The ligand L1 was dried over anhydrous MgSO4, filtered, concentrated, and column chromatography was performed to obtain a yield of 33%; 1 H NMR (500MHz, CDCl3, TMS): δ11.30(s,1H),7.72-7.67(m,4H),7.58-7.55(m,2H),7.49-7 .46(m,4H),6.74-6.70(m,1H),6.58-6.55(m,1H),2.74-2.68(m,4H),1.83-1.74(m,4H). 13 C NMR (126MHz, CDCl3) δ161.96,161.94,144.03,144.01,132.69,132.32,132.30,132.04,131.96,131.85,128.65,128.5 5,128.17,128.09,127.01,126.95,119.89,119.79,106.84,105.99,77.27,77.02,76.76,30.04,22.78,22.54,22.48. 31 P NMR (202MHz, CDCl3) δ 39.67;

[0194] In a nitrogen atmosphere, ligand L1 (0.66 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a tetrahydrofuran solution of TiCl4(THF)2 (0.334 g, 1 mmol) was added dropwise. The mixture was reacted at room temperature overnight, the solvent was drained, and dichloromethane (30 mL) was added to dissolve the mixture. The filter cake was removed by filtration, the filtrate was concentrated, and heptane was added for recrystallization to obtain complex 2 with a yield of 77%. The elemental analysis test showed that C 44 H 40Cl2O2P2Ti(781.52): Theoretical calculated values ​​are: C, 67.62; H, 5.16; Test values ​​are: C, 67.43; H, 5.33;

[0195] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2 was added, methylaluminoxane (6.5mL, 10mmol) was added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0196] Example 2

[0197] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0198] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2 was added, methylaluminoxane (6.5mL, 10mmol) was added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 10atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0199] Example 3

[0200] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0201] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2 was added, methylaluminoxane (6.5mL, 10mmol) was added, and the reaction was stirred vigorously at 80°C while maintaining an ethylene pressure of 10atm for 30min. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0202] Example 4

[0203] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0204] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2, 10mL of 1-octene, methylaluminoxane (6.5mL, 10mmol) were added, and the reaction was carried out at 30°C while maintaining an ethylene pressure of 1.0atm with vigorous stirring for 30min. The copolymer was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain the copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0205] Example 5

[0206] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0207] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2, 0.5g of norbornene, and methylaluminoxane (6.5mL, 10mmol) were added, and the reaction was carried out at 30°C while maintaining an ethylene pressure of 1.0atm and vigorously stirred for 10min. The copolymer was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain the copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0208] Example 6

[0209] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0210] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2, 0.5g of norbornene, and methylaluminoxane (6.5mL, 10mmol) were added, and the reaction was carried out at 50°C while maintaining an ethylene pressure of 1.0atm with vigorous stirring for 10min. The copolymer was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain the copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0211] Example 7

[0212] Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2;

[0213] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, 7.8mg (10μmol) of complex 2, 0.5g of norbornene, and methylaluminoxane (6.5mL, 10mmol) were added, and the reaction was carried out at 70°C while maintaining an ethylene pressure of 1.0atm and vigorously stirred for 10min. The copolymer was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain the copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0214] Example 8

[0215] Complex 21: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is Cl, n=2;

[0216] Ligand L1 was prepared according to the method of Example 1;

[0217] In a nitrogen atmosphere, ligand L1 (0.66 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a tetrahydrofuran solution (-78°C) of (THF)2ZrCl4 (0.38 g, 1 mmol) was added dropwise. The mixture was reacted at room temperature overnight, the solvent was drained, and dichloromethane (30 mL) was added to dissolve the mixture. The filter cake was removed by filtration, the filtrate was concentrated, and heptane was added for recrystallization to obtain complex 21 with a yield of 71%. The elemental analysis test showed that C 44 H 40 Cl2O2P2Zr (824.87): Theoretical calculated values ​​are: C, 64.07; H, 4.89; Test values ​​are: C, 63.79; H, 4.95;

[0218] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (6.5mL, 10mmol) and 8.2mg (10μmol) of complex 21 were added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0219] Example 9

[0220] Complex 36: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is Cl, n=2;

[0221] Ligand L1 was prepared according to the method of Example 1;

[0222] In a nitrogen atmosphere, ligand L1 (0.66 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered to remove the mixture, and a tetrahydrofuran solution (-78°C) of (THF)2HfCl4 (0.46 g, 1 mmol) was added dropwise. The mixture was reacted at room temperature overnight, the solvent was drained, and dichloromethane (30 mL) was added to dissolve the mixture. The filter cake was removed by filtration, the filtrate was concentrated, and heptane was added for recrystallization to obtain complex 36 with a yield of 76%. The elemental analysis test showed that C 44 H 40 Cl2O2P2Hf (912.14): Theoretical calculated values ​​are: C, 57.94; H, 4.42; Test values ​​are: C, 57.78; H, 4.31;

[0223] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (6.5mL, 10mmol) and 9.1mg (10μmol) of complex 36 were added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0224] Example 10

[0225] Complex 14: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 10 For H, R8 and R 10is -CF3, X is Cl, n=2;

[0226] In a nitrogen atmosphere, the compound represented by formula (III) (2.32 g, 10 mmol) was dissolved in anhydrous ether (20 mL), and n-butyl lithium solution (2.7 M, 4.0 mL, 11 mmol) was added dropwise at -78 °C. The reaction gradually returned to room temperature and continued to stir for 12 h to obtain a white precipitate. Bis(3,5-di(trifluoromethyl)phenyl)chlorophosphine (PPh2(CF3)4Cl) (11 mmol, 5.42 g) was evenly dispersed in 10 mL of ether and added dropwise to the original reaction system under an ice-water bath. The temperature was slowly raised to room temperature and stirred overnight. The mixture was quenched with water, and the organic phase was extracted with ether. The obtained organic phase was concentrated, deoxygenated by freezing cycle, and 5 mL of concentrated hydrochloric acid was added under a nitrogen atmosphere to react for 5 h. The reaction was followed by TLC to complete. Then, NaHCO3 aqueous solution was added for neutralization, quenched with water, and the organic phase was extracted with ether. The ligand L2 was dried over anhydrous MgSO4, filtered, concentrated, and column chromatography was performed to obtain the ligand L2 with a yield of 31%. 1 H NMR (500MHz, CDCl3, TMS): δ10.48 (s, 0.9H), 8.13-8.11 (d, J = 13.0Hz, 6H), 6.70-6.66 (m,2H),2.78-2.76(t,J=5.5Hz,2H),2.71-2.68(t,J=6.0Hz,2H),1.84-1.79(m,4H). 13 C NMR (126MHz, CDCl3) δ162.14,146.44,135.07,134.24,133.39,133.28,133. 00,132.90,132.73,132.63,132.46,132.36,131.80,131.78,131.71,131.6 8,128.33,128.26,126.92,126.89,126.86,126.84,126.82,126.74,123.64,121.46,121.36,121.25,77.28,77.02,76.77,30.14,22.75,22.26,22.20. 31 P NMR (202MHz, CDCl3) δ 34.86;

[0227] In a nitrogen atmosphere, ligand L2 (1.21 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a tetrahydrofuran solution of TiCl4(THF)2 (0.334 g, 1 mmol) was added dropwise. The mixture was reacted at room temperature overnight, the solvent was drained, and dichloromethane (30 mL) was added to dissolve the mixture. The filter cake was removed by filtration, the filtrate was concentrated, and heptane was added for recrystallization to obtain complex 14 with a yield of 75%. The elemental analysis test showed that C 52 H 32 Cl2F 24 O2P2Ti(1325.50): Theoretical calculated values ​​are: C, 47.12; H, 2.43; Test values ​​are: C, 47.01; H, 2.30;

[0228] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (3.3mL, 5mmol) and 6.6mg (5μmol) of complex 14 were added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0229] Embodiment 11

[0230] Complex 30: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 10 For H, R8 and R 10 is -CF3, X is Cl, n=2;

[0231] Ligand L2 was prepared according to the method of Example 10;

[0232] In a nitrogen atmosphere, ligand L2 (1.21 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a tetrahydrofuran solution of (THF)2ZrCl4 (0.38 g, 1 mmol) (-78°C) was added dropwise. The reaction was allowed to proceed overnight at room temperature, and the solvent was drained. Dichloromethane (30 mL) was added to dissolve the mixture, and the filter cake was removed by filtration. The filtrate was concentrated, and heptane was added for recrystallization to obtain complex 30 with a yield of 71%. The elemental analysis test showed that C 52 H 32 Cl2F 24 O2P2Zr (1368.86): Theoretical calculated values ​​are: C, 45.63; H, 2.36; Test values ​​are: C, 45.42; H, 2.30;

[0233] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (3.3mL, 5mmol) and 6.8mg (5μmol) of complex 30 were added, and the reaction was stirred vigorously for 30min at 30°C while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0234] Example 12

[0235] Complex 24: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is Cl, n=2;

[0236] In a nitrogen atmosphere, the compound represented by formula (III) (2.32 g, 10 mmol) was dissolved in 20 mL of anhydrous ether, and n-butyl lithium solution (2.7 M, 4.0 mL, 11 mmol) was added dropwise at -78 ° C. The reaction gradually returned to room temperature and continued to stir for 12 h to obtain a white precipitate. Di(4-methoxy)phosphine chloride (PPh2(OMe)2Cl) (11 mmol, 3.08 g) was evenly dispersed in 10 mL of ether and added dropwise to the original reaction system under an ice-water bath. The temperature was slowly raised to room temperature and stirred overnight. The mixture was quenched with water, and the organic phase was extracted with ether. The obtained organic phase was concentrated, deoxygenated by freezing cycle, and 5 mL of concentrated hydrochloric acid was added under a nitrogen atmosphere to react for 5 h. The reaction was followed by TLC to complete, and then a NaHCO3 aqueous solution was added for neutralization, quenched with water, and the organic phase was extracted with ether. The ligand L3 was dried over anhydrous MgSO4, filtered, concentrated, and column chromatography was performed to obtain the ligand L3 with a yield of 28%. The elemental analysis test was C 24 H 25 O3P (392.43): Theoretical calculated values ​​are: C, 73.46; H, 6.42; Test values ​​are: C, 73.15; H, 6.78;

[0237] In a nitrogen atmosphere, ligand L3 (0.78 g, 2 mmol) was dissolved in tetrahydrofuran, excess NaH (0.072 g, 3 mmol) was added, and the mixture was stirred at room temperature for 10 h. NaH was filtered out, and a tetrahydrofuran solution of (THF)2ZrCl4 (0.38 g, 1 mmol) (-78°C) was added dropwise. The reaction was allowed to proceed overnight at room temperature, and the solvent was drained. Dichloromethane (30 mL) was added to dissolve the mixture, and the filter cake was removed by filtration. The filtrate was concentrated, and heptane was added for recrystallization to obtain complex 24 with a yield of 77%. The elemental analysis test showed that C 48 H 48Cl2O6P2Zr (944.98): Theoretical calculated values ​​are: C, 61.01; H, 5.12; Test values ​​are: C, 61.25; H, 5.32;

[0238] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (3.3mL, 5mmol) and 4.7mg (5μmol) of complex 24 were added, and the reaction was carried out at 30°C while maintaining an ethylene pressure of 1.0atm and vigorously stirred for 30min. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0239] Comparative Example 1

[0240] A 1L stainless steel polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 500mL of toluene was injected into the polymerization kettle, methylaluminoxane (6.5mL, 10mmol) and 4.7mg (10μmol) of complex A (synthesis reference Organometallics, 2008, 27(2), 235-245) were added, and the reaction was stirred vigorously at 30°C for 30min while maintaining an ethylene pressure of 1.0atm. The reaction was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain polyethylene. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0241]

[0242] Comparative Example 2

[0243] A 100mL glass polymerization kettle equipped with mechanical stirring was dried continuously at 130°C for 6h, evacuated while hot and replaced with N2 gas three times, 50mL of toluene was injected into the polymerization kettle, methylaluminoxane (6.5mL, 10mmol), 0.5g of norbornene, 4.7mg (10μmol) of complex A were added, and the reaction was stirred vigorously for 10min at 30°C while maintaining an ethylene pressure of 1.0atm. The copolymer was neutralized with an ethanol solution acidified with 10wt% hydrochloric acid to obtain the copolymer. The polymer was dried and weighed to test the polymerization activity. The test data of the weight average molecular weight, molecular weight distribution and polymerization activity of the obtained polymer are shown in Table 1.

[0244] Table 1

[0245]

[0246]

[0247] It can be seen from the data in Table 1 that when the tetralinol-phosphine transition metal complex of the present invention is used as the main catalyst, under similar polymerization conditions, it has higher homopolymerization / copolymerization activity, the molecular weight of the obtained polymer is significantly improved, and the molecular weight distribution is narrower.

[0248] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A tetralinol-phosphine transition metal complex, characterized in that: Its structural formula is shown in formula (I), Wherein, M is selected from Group IVB metals; Ar is selected from substituted or unsubstituted C6-C20 aromatic groups; X is selected from halogen or C1-C10 hydrocarbon groups, and n is 1 or 2.

2. The tetralin-phosphine transition metal complex according to claim 1, characterized in that: Its structural formula is shown in formula (II), Among them, R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl and substituted or unsubstituted C1-C20 hydrocarbon group; Preferably, M is selected from Ti, Zr or Hf; Preferably, X is selected from halogen or C1-C8 hydrocarbon group, and n is 1 or 2.

3. The tetralin-phosphine transition metal complex according to claim 2, characterized in that: R7-R 11 Each is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C10 alkyl and substituted or unsubstituted C6-C15 aryl; Preferably, the substituent is selected from halogen, hydroxyl, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy or halogenated C1-C6 alkoxy; Preferably, the C1-C6 alkyl group is selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl or 3,3-dimethylbutyl; Preferably, the C1-C6 alkoxy group is selected from methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy or 3,3-dimethylbutoxy; Preferably, the halogen is selected from fluorine, chlorine, bromine or iodine.

4. The tetralin-phosphine transition metal complex according to any one of claims 1 to 3, characterized in that: It is selected from the group consisting of the following complexes: Complex 1: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=1; Complex 2: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is Cl, n=2; Complex 3: A complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is methyl, n=2; Complex 4: Complex represented by formula (II), wherein M is Ti, R7-R 11 is H, X is -CH2C6H5, n=2; Complex 5: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is Cl, and n=1; Complex 6: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is Cl, n=2; Complex 7: A complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2; Complex 8: Complex represented by formula (II), wherein M is Ti, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2; Complex 9: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=1; Complex 10: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2; Complex 11: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2; Complex 12: A complex represented by formula (II), wherein M is Ti, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2; Complex 13: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=1; Complex 14: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2; Complex 15: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2; Complex 16: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2; Complex 17: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=1; Complex 18: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2; Complex 19: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2; Complex 20: A complex represented by formula (II), wherein M is Ti, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, n=2; Complex 21: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is Cl, n=2; Complex 22: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is methyl, n=2; Complex 23: A complex represented by formula (II), wherein M is Zr, R7-R 11 is H, X is -CH2C6H5, n=2; Complex 24: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is Cl, n=2; Complex 25: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2; Complex 26: A complex represented by formula (II), wherein M is Zr, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2; Complex 27: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2; Complex 28: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2; Complex 29: A complex represented by formula (II), wherein M is Zr, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2; Complex 30: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2; Complex 31: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2; Complex 32: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2; Complex 33: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2; Complex 34: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2; Complex 35: A complex represented by formula (II), wherein M is Zr, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, n=2; Complex 36: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is Cl, n=2; Complex 37: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is methyl, n=2; Complex 38: A complex represented by formula (II), wherein M is Hf, R7-R 11 is H, X is -CH2C6H5, n=2; Complex 39: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is Cl, n=2; Complex 40: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is methyl, and n=2; Complex 41: A complex represented by formula (II), wherein M is Hf, R8-R 11 is H, R7 is methoxy, X is -CH2C6H5, n=2; Complex 42: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is Cl, n=2; Complex 43: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is methyl, and n=2; Complex 44: A complex represented by formula (II), wherein M is Hf, R7, R8, R 10 and R 11 is H, R9 is methoxy, X is -CH2C6H5, n=2; Complex 45: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is Cl, n=2; Complex 46: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is methyl, n=2; Complex 47: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is -CF3, X is -CH2C6H5, n=2; Complex 48: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is Cl, n=2; Complex 49: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is a methyl group, X is a methyl group, and n=2; Complex 50: A complex represented by formula (II), wherein M is Hf, R7, R9 and R 11 For H, R8 and R 10 is methyl, X is -CH2C6H5, and n=2.

5. A method for preparing the tetrahydronaphthol-phosphine transition metal complex as claimed in any one of claims 1 to 4, characterized in that: The method includes: (1) reacting the compound represented by formula (III) with the compound represented by formula (IV) to generate a ligand; (2) reacting the ligand with a second hydrogen extraction agent, and then reacting with an M metal compound; Wherein, the metal M in the M metal compound is selected from Group IVB metals, and the definition of Ar is the same as that in claim 1.

6. The method according to claim 5, characterized in that The M metal compound is selected from one or more of titanium tetrachloride, bis(tetrahydrofuran)titanium tetrachloride, tri(tetrahydrofuran)titanium trichloride, zirconium tetrachloride, bis(tetrahydrofuran)zirconium tetrachloride, hafnium tetrachloride and bis(tetrahydrofuran)hafnium tetrachloride; Preferably, the second hydrogen extraction agent is selected from one or more of NaH, KH, n-butyl lithium and methyl lithium.

7. Use of the tetralinol-phosphine transition metal complex according to any one of claims 1 to 4 in olefin polymerization.

8. A catalyst for olefin polymerization, characterized in that The olefin polymerization catalyst comprises a main catalyst and a co-catalyst; The main catalyst is the tetralin-phosphine pre-transition metal complex described in any one of claims 1 to 4.

9. The catalyst for olefin polymerization according to claim 8, characterized in that The co-catalyst is an organoaluminum compound and / or an organoboron compound; Preferably, the organoaluminum compound is selected from alkylaluminoxanes or organoaluminum compounds having the general formula AlY n Z 3-n , wherein Y is selected from hydrogen, C1-C20 hydrocarbon groups or C1-C20 alkoxy groups, Z is selected from halogens, 0 < n ≤ 3, and n is an integer; Preferably, Y is selected from C1-C20 alkyl, C1-C20 alkoxy, C7-C20 aralkyl or C6-C20 aryl; Preferably, Z is selected from chlorine or bromine; Preferably, the organic boron compound is selected from aromatic boron and / or organic borate.

10. Use of the catalyst for olefin polymerization according to claim 8 or 9 in olefin polymerization.

11. An olefin polymerization method, characterized in that: The method comprises carrying out an olefin polymerization reaction in the presence of the olefin polymerization catalyst according to claim 8 or 9; Preferably, the polymerization reaction temperature is -78°C to 200°C, more preferably -20°C to 150°C; the polymerization pressure is 0.01 to 10 MPa, more preferably 0.01 to 5 MPa.

Citation Information

Cited By

  • Tetrahydronaphthol-phosphine pre-transition metal complex, and preparation method therefor and use thereof

    EP4707283A1