Polytetrafluoroethylene microporous membrane, preparation method thereof and proton exchange membrane
By using fluorocarbon hybrid surfactant in the proton exchange membrane to improve the hydrophilicity and compatibility of the polytetrafluoroethylene microporous membrane, the performance problems of the proton exchange membrane under different humidity conditions are solved, and the fuel cell is improved Performance and lifespan.
Patent Information
- Application Number
- CN202411209021.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The volume changes of the existing proton exchange membrane under different humidity conditions affect the interface binding force between it and the electrode, resulting in a decrease in fuel cell performance and life. The proton conductivity of the enhanced composite membrane is insufficient, so it is necessary to improve the hydrophilicity of the ePTFE membrane. to improve compatibility.
Using fluorocarbon hybrid surfactant, pre-pressing, extrusion, calendering, stretching and sintering is performed by mixing with PTFE resin powder and lubricating oil to prepare a polytetrafluoroethylene microporous membrane to improve its hydrophilicity and completeness. The wetting property of the fluorosulfonic acid resin can improve the ion conduction efficiency and mechanical durability of the proton exchange membrane.
It significantly improves the hydrophilicity and processing performance of the PTFE microporous membrane, enhances compatibility with perfluorosulfonic acid resin, improves the ion conduction efficiency and mechanical durability of the proton exchange membrane, prevents hydrogen leakage, and improves the The performance and durability of fuel cells are achieved.
Smart Images

Figure CN119081182A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a polytetrafluoroethylene microporous membrane and a preparation method thereof, and further relates to a proton exchange membrane. Background Art
[0002] As energy demand continues to rise, this has prompted in-depth research and development of clean and sustainable new energy technologies around the world. Among them, proton exchange membrane fuel cells (PEMFC) have attracted widespread attention from the scientific research and industrial communities due to their significant advantages such as simple structure, low operating temperature and high efficiency. In PEMFC, the proton exchange membrane is placed between the electrodes to form a membrane electrode assembly, which not only provides a transmission path for protons, but also effectively prevents the crossover of hydrogen between the anode and the cathode. The commonly used proton exchange membrane material is Nafion, which is a perfluorosulfonic acid ionomer. The Nafion membrane achieves the transmission of protons in the form of ion clusters through phase separation between its hydrophilic sulfonic acid side chains and hydrophobic carbon fluoride main chains, thereby showing excellent chemical stability and high ionic conductivity.
[0003] However, the volume change of the proton exchange membrane under different humidity conditions will have an adverse effect on the interfacial bonding force between it and the electrode, which has become one of the challenges to improving the performance of fuel cells. To address this problem, researchers proposed the use of enhanced composite membranes, which impregnate ionic polymers into the porous support layer of expanded polytetrafluoroethylene (ePTFE), aiming to utilize the mechanical stability of ePTFE and the conductivity of ionic polymers to improve the overall performance of the proton exchange membrane. However, the hydrophilicity of ePTFE is poor, which makes the proton conductivity of the enhanced composite membrane insufficient and needs to be further improved. Summary of the invention
[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: Due to the compatibility problem between the hydrophilic ionic polymer and the extremely hydrophobic ePTFE membrane, the ionic polymer cannot be completely impregnated on the ePTFE membrane, which not only reduces the conductivity of protons, but also may increase the permeability of hydrogen, thereby affecting the performance and life of the fuel cell. In view of this, it is necessary to conduct in-depth research to improve the hydrophilicity of the ePTFE membrane and improve the compatibility of the ePTFE membrane with the ionic polymer, thereby improving the performance of the proton exchange membrane.
[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the embodiments of the present invention provide a polytetrafluoroethylene microporous membrane and a preparation method thereof, which effectively improves the hydrophilicity of the polytetrafluoroethylene microporous membrane and enhances the wettability between the polytetrafluoroethylene microporous membrane and the perfluorosulfonic acid resin, thereby helping to improve the ion conduction efficiency and durability of the proton exchange membrane.
[0006] The method for preparing the polytetrafluoroethylene microporous membrane according to the embodiment of the present invention comprises the following steps:
[0007] a. Preparation of a fluorocarbon hybrid surfactant: 2,2,3,3,3-pentafluoro-1-propanol, a phase transfer catalyst, an organic solvent, and a first alkaline catalyst are mixed, glycidyl ether is added, and a first reaction is performed to obtain an intermediate product, wherein the glycidyl ether includes at least one of butyl glycidyl ether and octyl glycidyl ether; the intermediate product, a second alkaline catalyst, and ethylene oxide are mixed in a reactor, and a second reaction is performed to obtain a fluorocarbon hybrid surfactant;
[0008] b. Mixing PTFE resin powder, lubricating oil and the fluorocarbon hybrid surfactant obtained in step a, and preparing a polytetrafluoroethylene microporous membrane through pre-pressing, extruding, calendering, stretching and sintering.
[0009] Advantages and technical effects brought by the preparation method of polytetrafluoroethylene microporous membrane of the embodiment of the present invention: 1. In the method of the embodiment of the present invention, the introduction of fluorocarbon hybrid surfactant can effectively reduce the friction between polytetrafluoroethylene (PTFE) resin particles, improve the uniformity of particle mixing, and prevent the resin from prematurely fiberizing during processing; 2. In the method of the embodiment of the present invention, by introducing fluorocarbon hybrid surfactant, the processing performance of the material is significantly improved, making it easier to be formed by extrusion and stretching processes; 3. In the method of the embodiment of the present invention, the introduced fluorocarbon hybrid surfactant has excellent wettability, which not only effectively improves the hydrophilicity of the ePTFE membrane, but also enhances the bond between ePTFE and perfluorosulfonic acid resin. The main reason is that the surfactant contains fluorocarbon side chains, hydrocarbon side chains and non-ionic ethylene oxide chains. Since PTFE is non-polar and perfluorosulfonic acid resin solution is usually polar, the wettability between the two is poor. The hydrocarbon part of the surfactant prepared in the embodiment of the present invention can interact with the non-polar PTFE membrane, while the fluorocarbon and ethylene oxide parts can interact with the polar perfluorosulfonic acid resin solution, thereby improving the compatibility between the two, thereby improving the ion conduction efficiency and mechanical durability of the proton exchange membrane, and can prevent hydrogen leakage, improve the performance and durability of the fuel cell, ensure the stable operation of the fuel cell under various working conditions, and show higher energy efficiency and longer service life.
[0010] In some embodiments, in step a, the molar ratio of the 2,2,3,3,3-pentafluoro-1-propanol and glycidyl ether is (1-1.4):1; the molar ratio of the first alkaline catalyst to 2,2,3,3,3-pentafluoro-1-propanol is 2-4:1; the molar ratio of the first alkaline catalyst to the phase transfer catalyst is (300-450):1; the molar ratio of ethylene oxide to 2,2,3,3,3-pentafluoro-1-propanol is (8-15):1; the molar ratio of ethylene oxide to the second alkaline catalyst is (100-200):1.
[0011] In some embodiments, in step a, the first alkaline catalyst includes at least one of sodium hydroxide or potassium hydroxide solid; the phase transfer catalyst includes at least one of tetrabutylammonium bromide and tetrabutylammonium chloride; the second alkaline catalyst includes at least one of sodium hydroxide or potassium hydroxide solid; and the organic solvent includes at least one of toluene, xylene, and ethylbenzene.
[0012] In some embodiments, in step a, the reaction temperature of the first reaction is 60-80°C, and the reaction time is 20-30h; the reaction temperature of the second reaction is 80-100°C, and the reaction time is 2-6h.
[0013] In some embodiments, in step a, after the second reaction is completed, the reaction mixture is dissolved in chloroform, washed with distilled water until neutral, dried with anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a fluorocarbon hybrid surfactant.
[0014] In some embodiments, in the step b, the fluorocarbon hybrid surfactant is added to the lubricating oil, magnetically stirred for 5-10 minutes, and then PTFE resin powder is added, left to stand, matured, and pre-pressed to form a preform, the pre-pressing pressure is 5-10MPa, and the pre-pressing time is 10-20min; the extrusion temperature is 50-80°C, the extrusion speed is 60-100mm / min, and a rod-shaped material is extruded; the thickness of the calendered film obtained by calendering is 200-400μm; the stretching includes longitudinally stretching the calendered film obtained by calendering by 500% to 1000% at 200-300°C, and then transversely stretching it by 1000% to 4000% at 200-300°C; the sintering temperature is 330-360°C.
[0015] In some embodiments, in step b, the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil, and liquid paraffin; and the particle size of the PTFE resin powder is 400-600 nm.
[0016] In some embodiments, in step b, the mass of the lubricating oil is 20-30% of the mass of the PTFE resin powder; the mass of the fluorocarbon hybrid surfactant is 0.5-3% of the mass of the PTFE resin powder.
[0017] The embodiment of the present invention also provides a polytetrafluoroethylene microporous membrane, which is prepared by the method of the embodiment of the present invention. The polytetrafluoroethylene microporous membrane of the embodiment of the present invention has good hydrophilicity and excellent wettability with perfluorosulfonic acid resin, which is beneficial to improving the ion conduction efficiency and mechanical durability of the proton exchange membrane, and can prevent hydrogen leakage, thereby improving the performance and durability of the fuel cell.
[0018] The present invention also provides a proton exchange membrane, including a polytetrafluoroethylene microporous membrane prepared by the method of the present invention or a polytetrafluoroethylene microporous membrane of the present invention. The proton exchange membrane of the present invention has all the advantages that the polytetrafluoroethylene microporous membrane of the present invention can bring, which will not be repeated here. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is an electron microscope spectrum of the polytetrafluoroethylene microporous membrane of Example 1.
[0020] Figure 2 Schematic diagram of water contact angle of polytetrafluoroethylene microporous membranes in various embodiments and comparative examples. DETAILED DESCRIPTION
[0021] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0022] The method for preparing the polytetrafluoroethylene microporous membrane according to the embodiment of the present invention comprises the following steps:
[0023] a. Preparation of a fluorocarbon hybrid surfactant: 2,2,3,3,3-pentafluoro-1-propanol, a phase transfer catalyst, an organic solvent, and a first alkaline catalyst are mixed, glycidyl ether is added, and a first reaction is performed to obtain an intermediate product, wherein the glycidyl ether includes at least one of butyl glycidyl ether and octyl glycidyl ether; the intermediate product, a second alkaline catalyst, and ethylene oxide are mixed in a reactor, and a second reaction is performed to obtain a fluorocarbon hybrid surfactant;
[0024] b. Mixing PTFE resin powder, lubricating oil and the fluorocarbon hybrid surfactant obtained in step a, and preparing a polytetrafluoroethylene microporous membrane through pre-pressing, extruding, calendering, stretching and sintering.
[0025] In the preparation method of the polytetrafluoroethylene microporous membrane of the embodiment of the present invention, a fluorocarbon hybrid surfactant is introduced, which can effectively reduce the friction between polytetrafluoroethylene (PTFE) resin particles, improve the uniformity of particle mixing, and prevent the resin from prematurely fiberizing during processing; in the method of the embodiment of the present invention, by introducing a fluorocarbon hybrid surfactant, the processing performance of the material is significantly improved, making it easier to form through extrusion and stretching processes; in the method of the embodiment of the present invention, the introduced fluorocarbon hybrid surfactant has excellent wettability, which not only effectively improves the hydrophilicity of the ePTFE membrane, but also enhances the wettability between the ePTFE and the perfluorosulfonic acid resin, which is mainly due to Because the surfactant contains fluorocarbon side chains, hydrocarbon side chains and non-ionic ethylene oxide chains, and since PTFE is non-polar and perfluorosulfonic acid resin solution is usually polar, the wettability between the two is poor. The hydrocarbon part of the surfactant prepared in the embodiment of the present invention can interact with the non-polar PTFE membrane, while the fluorocarbon and ethylene oxide parts can interact with the polar perfluorosulfonic acid resin solution, thereby improving the compatibility of the two, thereby improving the ion conduction efficiency and mechanical durability of the proton exchange membrane, and can prevent hydrogen leakage, improve the performance and durability of the fuel cell, ensure the stable operation of the fuel cell under various working conditions, and show higher energy efficiency and longer service life.
[0026] In some embodiments, in step a, the molar ratio of 2,2,3,3,3-pentafluoro-1-propanol to glycidyl ether is (1-1.4): 1. In the embodiment of the present invention, 2,2,3,3,3-pentafluoro-1-propanol and glycidyl ether react to generate an intermediate product, a fluoroalcohol derivative. For example, when the glycidyl ether is butyl glycidyl ether, the generated intermediate product is: 1-butoxy-3-(2,2,3,3,3-pentafluoropropoxy)propan-2-ol. In the embodiment of the present invention, the ratio between 2,2,3,3,3-pentafluoro-1-propanol and glycidyl ether is preferably selected, so that each substance can fully react to obtain an intermediate product. If too much 2,2,3,3,3-pentafluoro-1-propanol is added, it will exist as an impurity in the final product, affecting the purity and effect of the product. If too little 2,2,3,3,3-pentafluoro-1-propanol is added, the excess glycidyl ether will undergo side reactions such as ring opening and polymerization, which is not conducive to improving the yield of the expected product.
[0027] In some embodiments, in step a, the molar ratio of the first alkaline catalyst to 2,2,3,3,3-pentafluoro-1-propanol is 2-4:1, and preferably, the first alkaline catalyst comprises at least one of sodium hydroxide or potassium hydroxide solid. In the embodiment of the present invention, a strong base catalyst is added to promote the Williamson reaction of 2,2,3,3,3-pentafluoro-1-propanol and glycidyl ether. If the first alkaline catalyst is too much, side reactions will occur, reducing the yield of the target product. If the first alkaline catalyst is too little, the catalyst cannot effectively play its role, which will slow down the reaction rate.
[0028] In some embodiments, the molar ratio of the first alkaline catalyst to the phase transfer catalyst is (300-450): 1. Preferably, the phase transfer catalyst comprises at least one of tetrabutylammonium bromide and tetrabutylammonium chloride. In the embodiments of the present invention, the phase transfer catalyst and its dosage are preferably selected to effectively promote the dissolution of the first alkaline catalyst in the organic solvent.
[0029] In some embodiments, in step a, the molar ratio of ethylene oxide to 2,2,3,3,3-pentafluoro-1-propanol is (8-15):1; the molar ratio of ethylene oxide to the second alkaline catalyst is (100-200):1, preferably, the second alkaline catalyst comprises at least one of sodium hydroxide or potassium hydroxide solid. In the embodiment of the present invention, the intermediate product and ethylene oxide continue to react to form a fluorocarbon hybrid surfactant. In the embodiment of the present invention, the amount of ethylene oxide is preferably selected. If too much ethylene oxide is added, side reactions such as ring opening and polymerization of ethylene oxide will occur, which is not conducive to the formation of the expected product fluorocarbon hybrid surfactant; if too little ethylene oxide is added, the molecular weight distribution of the product will become broad, which is not conducive to improving the use effect of the surfactant.
[0030] In some embodiments, in step a, the organic solvent comprises at least one of toluene, xylene and ethylbenzene. In the embodiment of the present invention, the addition of the organic solvent provides a uniform reaction environment for the reaction raw materials.
[0031] In some embodiments, in step a, the reaction temperature of the first reaction is 60-80°C, and the reaction time is 20-30h; the reaction temperature of the second reaction is 80-100°C, and the reaction time is 2-6h.
[0032] In some embodiments, in step a, after the second reaction is completed, the reaction mixture is dissolved in chloroform, washed with distilled water until neutral, dried with anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a fluorocarbon hybrid surfactant.
[0033] In some embodiments, in the step b, the fluorocarbon hybrid surfactant is added to the lubricating oil, magnetically stirred for 5-10 minutes, and then PTFE resin powder is added, left to stand, matured, and pre-pressed to form a preform, the pre-pressing pressure is 5-10MPa, and the pre-pressing time is 10-20min; the extrusion temperature is 50-80°C, the extrusion speed is 60-100mm / min, and a rod-shaped material is extruded; the thickness of the calendered film obtained by calendering is 200-400μm; the stretching includes longitudinally stretching the calendered film obtained by calendering by 500% to 1000% at 200-300°C, and then transversely stretching it by 1000% to 4000% at 200-300°C; the sintering temperature is 330-360°C.
[0034] In some embodiments, in step b, the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil, and liquid paraffin; and the particle size of the PTFE resin powder is 400-600 nm.
[0035] In some embodiments, in step b, the mass of the lubricating oil is 20-30% of the mass of the PTFE resin powder.
[0036] In some embodiments, in step b, the mass of the fluorocarbon hybrid surfactant is 0.5-3% of the mass of the PTFE resin powder. In the embodiments of the present invention, the amount of the fluorocarbon hybrid surfactant added is preferably selected. If too little is added, the fluorocarbon hybrid surfactant has little effect on improving the hydrophilicity of the polytetrafluoroethylene microporous membrane. If too much is added, the mechanical properties of the polytetrafluoroethylene microporous membrane will be reduced.
[0037] The embodiment of the present invention also provides a polytetrafluoroethylene microporous membrane, which is prepared by the method of the embodiment of the present invention. The polytetrafluoroethylene microporous membrane of the embodiment of the present invention has good hydrophilicity and excellent wettability with perfluorosulfonic acid resin, which is beneficial to improving the ion conduction efficiency and mechanical durability of the proton exchange membrane, and can prevent hydrogen leakage, thereby improving the performance and durability of the fuel cell.
[0038] The present invention also provides a proton exchange membrane, including a polytetrafluoroethylene microporous membrane prepared by the method of the present invention or a polytetrafluoroethylene microporous membrane of the present invention. The proton exchange membrane of the present invention has all the advantages that the polytetrafluoroethylene microporous membrane of the present invention can bring, which will not be repeated here.
[0039] The present invention is described in detail below with reference to the embodiments and the accompanying drawings.
[0040] Example 1
[0041] (I) Preparation of polytetrafluoroethylene microporous membrane
[0042] 1. Add 0.11mol 2,2,3,3,3-pentafluoro-1-propanol, 0.6mmol tetrabutylammonium bromide and 120ml toluene into a three-necked round flask, add 0.25mol sodium hydroxide into the three-necked round flask under constant stirring, and finally add 0.1mol butyl glycidyl ether into the flask slowly with a dropping funnel, and react at 70°C for 24h to obtain an intermediate product. Add the intermediate product and 0.01mol KOH into an autoclave at 80-100°C, add 1mol ethylene oxide, and react for 4h under stirring. After the reaction, place the mixture into a separating funnel, dissolve in 120mL chloroform, wash with distilled water until neutral, add anhydrous sodium sulfate to dry, and finally filter and concentrate under reduced pressure to obtain the target fluorocarbon hybrid surfactant.
[0043] 2. Add 0.5% of fluorocarbon hybrid surfactant (i.e., the fluorocarbon hybrid surfactant is 0.5% of the mass of PTFE resin) to 25% of isoparaffin lubricating oil (i.e., the lubricating oil is 25% of the mass of PTFE resin), stir on a magnetic stirrer for 5 minutes, mix the mixture of fluorocarbon hybrid surfactant and lubricating oil with PTFE resin powder evenly, let it stand at 60°C, mature for 24 hours to form a paste, and pre-press the matured PTFE paste through a preforming device to form a preform, the pre-pressing pressure is 10 MPa, and the pre-pressing time is 10 minutes.
[0044] 3. The preform is extruded through an extruder at an extrusion temperature of 60°C and an extrusion speed of 60 mm / min to obtain a rod-shaped material, and the rod is calendered into a thin sheet through a calender. After high-temperature degreasing at 160°C to remove the lubricating oil, a 300 μm thick calendered film is obtained.
[0045] 4. The calendered film is sent to a stretching unit, first stretched 800% longitudinally at 220°C, then stretched 2000% transversely at 280°C, and finally sintered at 340°C to obtain a polytetrafluoroethylene microporous membrane.
[0046] like Figure 1 As shown, by observing the surface structure of the ePTFE membrane under a scanning electron microscope, it can be seen that the fibers are interwoven into a network, and the average diameter of a single fiber is about 80 nm.
[0047] 2. Preparation of Proton Exchange Membrane
[0048] First, a layer of perfluorosulfonic acid resin solution with a wet thickness of 120 μm was scraped on the coating machine, and then the polytetrafluoroethylene microporous membrane prepared in this embodiment was cut and covered thereon, and then a layer of perfluorosulfonic acid resin solution with a wet thickness of 80 μm was scraped and coated again. After waiting for 5 minutes, the wet membrane was placed in a 160° C. oven and dried for 10 minutes to obtain a proton exchange membrane.
[0049] The thickness of the ePTFE membrane prepared in this embodiment is 9 μm, and the thickness of the proton exchange membrane is 11.7 μm.
[0050] Example 2
[0051] The method is the same as that of Example 1, except that in step 2 of preparing the polytetrafluoroethylene microporous membrane, the amount of the fluorocarbon hybrid surfactant added is 1% of the mass of the PTFE resin.
[0052] The thickness of the ePTFE membrane prepared in this embodiment is 9.3 μm, and the thickness of the proton exchange membrane is 12.3 μm.
[0053] Example 3
[0054] The method is the same as that of Example 1, except that in step 2 of preparing the polytetrafluoroethylene microporous membrane, the amount of the fluorocarbon hybrid surfactant added is 2% of the mass of the PTFE resin.
[0055] The thickness of the ePTFE membrane prepared in this embodiment is 9.6 μm, and the thickness of the proton exchange membrane is 11.9 μm.
[0056] Example 4
[0057] The method is the same as that of Example 1, except that in step 2 of preparing the polytetrafluoroethylene microporous membrane, the amount of the fluorocarbon hybrid surfactant added is 3% of the mass of the PTFE resin.
[0058] The thickness of the ePTFE membrane prepared in this embodiment is 8.9 μm, and the thickness of the proton exchange membrane is 11.9 μm.
[0059] Example 5
[0060] The method is the same as that of Example 1, except that in step 4 of preparing the polytetrafluoroethylene microporous membrane, the longitudinal stretching is 1000% and the transverse stretching is 2500%.
[0061] The thickness of the ePTFE membrane prepared in this embodiment is 7.9 μm, and the thickness of the proton exchange membrane is 12.0 μm.
[0062] Example 6
[0063] The method is the same as that of Example 1, except that the glycidyl ether used in step 1 of preparing the polytetrafluoroethylene microporous membrane is octyl glycidyl ether.
[0064] The thickness of the ePTFE membrane prepared in this embodiment is 8.7 μm, and the thickness of the proton exchange membrane is 11.9 μm.
[0065] Comparative Example 1
[0066] The method is the same as that of Example 1, except that in the preparation of the polytetrafluoroethylene microporous membrane, step 1 is eliminated and no fluorocarbon hybrid surfactant is added in step 2.
[0067] Comparative Example 2
[0068] The method is the same as that of Example 1, except that in step 1 of preparing the polytetrafluoroethylene microporous membrane, the glycidyl ether is methyl glycidyl ether.
[0069] Comparative Example 3
[0070] The method is the same as that of Example 1, except that step 1 is eliminated and the surfactant added in step 2 is a commercially available ASAHIGUARD AG-7600 perfluoro surfactant.
[0071] The hydrophilicity test of the polytetrafluoroethylene microporous membranes of the embodiments and comparative examples was carried out. Figure 2 As shown, compared with Comparative Example 1, the water contact angle of the polytetrafluoroethylene microporous membrane is significantly reduced in each embodiment of the present application due to the introduction of the fluorocarbon hybrid surfactant, indicating that the fluorocarbon hybrid surfactant effectively improves the hydrophilicity of the polytetrafluoroethylene microporous membrane, especially the polytetrafluoroethylene microporous membrane of Example 3, the water contact angle is reduced to 108°.
[0072] The ePTFE membranes and proton exchange membranes prepared in the embodiments and comparative examples were subjected to performance tests. The test results are shown in Tables 1 and 2.
[0073] Tensile strength: The test equipment is a universal testing machine. A punching machine is used to cut the sample along the TD and MD directions of the sample. The sample width is 6 mm, the tensile rate is 50 mm / min, and the tensile strength is calculated in accordance with GB / T13022-1991.
[0074] Through conductivity: The test equipment is an AC impedance film test system. A punching machine is used to cut a 1 cm×3 cm rectangular film sample. The test is started after the temperature and humidity (80° C., 80% RH) reach the set values.
[0075] Hydrogen permeation current density: The test equipment is a test platform built in the laboratory. The proton membrane is cut into 10cm×10cm membrane samples. High-purity N2 and H2 with 100% RH humidification are introduced into the cathode and anode of the fuel cell respectively. The test conditions are: temperature 75℃, applied voltage range 0~5V. The hydrogen permeation current density can characterize the durability of the proton exchange membrane and is preferably controlled at 4.0mA / cm 2 The lower the value, the less hydrogen permeation, the longer the life of the proton exchange membrane, and the better the durability.
[0076] Table 1 ePTFE membrane performance test
[0077] Thickness(μm) Average pore size (nm) Porosity (%) Tensile strength(MPa) Example 1 9.0 197 70 72 Example 2 9.3 203 73 75 Example 3 9.6 210 78 80 Example 4 8.9 205 75 75 Example 5 7.9 199 71 81 Example 6 8.7 196 73 79 Comparative Example 1 9.2 185 62 65 Comparative Example 2 9.5 192 67 70 Comparative Example 3 8.9 201 68 72
[0078] Table 2 Proton exchange membrane performance test
[0079]
[0080] It can be seen from Table 1 and Table 2 that in the method of the embodiment of the present invention, by adding a fluorocarbon hybrid surfactant, the hydrophilicity of the polytetrafluoroethylene microporous membrane is effectively improved, and the tensile strength of the polytetrafluoroethylene microporous membrane is increased. At the same time, the wettability of the polytetrafluoroethylene microporous membrane and the perfluorosulfonic acid resin is also improved, the through conductivity and mechanical properties of the prepared proton exchange membrane are improved, and the hydrogen permeation current of the proton exchange membrane is reduced, and the durability of the proton exchange membrane is improved. The through conductivity of the proton exchange membrane can reach more than 0.10S / cm, the tensile strength can reach more than 55MPa, and the hydrogen permeation current can reach more than 4.0mA / cm 2 The following has excellent performance.
[0081] In Comparative Example 1, the fluorocarbon hybrid surfactant prepared in the embodiment of the present invention was not added. The average pore size and porosity of the polytetrafluoroethylene microporous membrane were significantly reduced compared with those in Example 1, and the wettability with the perfluorosulfonic acid resin was poor. At the same time, the mechanical properties also showed a decrease. The conductivity of the prepared proton exchange membrane decreased to 0.071S / cm, and the hydrogen permeation current density was as high as 4.75mA / cm 2 , durability is poor.
[0082] In Comparative Example 2, methyl glycidyl ether was used to react and prepare a fluorocarbon hybrid surfactant. Since the hydrocarbon group in methyl glycidyl ether is relatively short, the interaction between the surfactant and the ePTFE membrane is reduced, and the membrane surface cannot be effectively filled and covered as the longer hydrocarbon group in the glycidyl ether used in the embodiment of the present invention. As a result, the hydrophilicity, average pore size, porosity and tensile strength of the prepared polytetrafluoroethylene microporous membrane are all decreased compared with those in Example 1, and the wettability with perfluorosulfonic acid resin is insufficient, resulting in the through conductivity of the prepared proton exchange membrane being reduced to 0.089S / cm, and the hydrogen permeation current density being increased to 4.29mA / cm 2 , durability is significantly reduced.
[0083] In Comparative Example 3, the commercially available ASAHIGUARD AG-7600 perfluoro surfactant was used. Although the mechanical properties of the obtained polytetrafluoroethylene microporous membrane were comparable to those of Example 1 and the average pore size was higher than that of Example 1, the through conductivity of the obtained proton exchange membrane was only 0.091 S / cm, and the hydrogen permeation current density increased significantly to 4.35 mA / cm 2 , durability is poor.
[0084] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0085] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a polytetrafluoroethylene microporous membrane, characterized in that: The steps include: a. Preparation of a fluorocarbon hybrid surfactant: 2,2,3,3,3-pentafluoro-1-propanol, a phase transfer catalyst, an organic solvent, and a first alkaline catalyst are mixed, glycidyl ether is added, and a first reaction is performed to obtain an intermediate product, wherein the glycidyl ether includes at least one of butyl glycidyl ether and octyl glycidyl ether; the intermediate product, a second alkaline catalyst, and ethylene oxide are mixed in a reactor, and a second reaction is performed to obtain a fluorocarbon hybrid surfactant; b. Mixing PTFE resin powder, lubricating oil and the fluorocarbon hybrid surfactant obtained in step a, and preparing a polytetrafluoroethylene microporous membrane through pre-pressing, extruding, calendering, stretching and sintering.
2. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: In the step a, the molar ratio of 2,2,3,3,3-pentafluoro-1-propanol to glycidyl ether is (1-1.4):1; and / or, the molar ratio of the first alkaline catalyst to 2,2,3,3,3-pentafluoro-1-propanol is 2-4:1; And / or, the molar ratio of the first alkaline catalyst to the phase transfer catalyst is (300-450):1; and / or, the molar ratio of ethylene oxide to 2,2,3,3,3-pentafluoro-1-propanol is (8-15):1; And / or, the molar ratio of the ethylene oxide to the second alkaline catalyst is (100-200):
1.
3. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1 or 2, characterized in that: In the step a, the first alkaline catalyst comprises at least one of sodium hydroxide or potassium hydroxide solid; And / or, the phase transfer catalyst comprises at least one of tetrabutylammonium bromide and tetrabutylammonium chloride; and / or, the second alkaline catalyst comprises at least one of sodium hydroxide or potassium hydroxide solid; And / or, the organic solvent includes at least one of toluene, xylene, and ethylbenzene.
4. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1 or 2, characterized in that: In the step a, the reaction temperature of the first reaction is 60-80° C., and the reaction time is 20-30 h; and / or, the reaction temperature of the second reaction is 80-100° C., and the reaction time is 2-6 h.
5. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1 or 2, characterized in that: In the step a, after the second reaction is completed, the reaction mixture is dissolved in chloroform, washed with distilled water until neutral, dried by adding anhydrous sodium sulfate, filtered, and concentrated under reduced pressure to obtain a fluorocarbon hybrid surfactant.
6. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: In the step b, the fluorocarbon hybrid surfactant is added to the lubricating oil, and magnetic stirring is performed for 5-10 minutes, and then the PTFE resin powder is added, allowed to stand, mature, and pre-pressed to form a preform, wherein the pre-pressing pressure is 5-10 MPa and the pre-pressing time is 10-20 minutes; And / or, the extrusion temperature is 50-80°C, the extrusion speed is 60-100 mm / min, and a rod-shaped material is obtained by extrusion; And / or, the calendered film obtained by calendering has a thickness of 200-400 μm; And / or, the stretching comprises longitudinally stretching the calendered film obtained by calendering by 500% to 1000% at 200 to 300° C., and then transversely stretching the calendered film by 1000% to 4000% at 200 to 300° C.; And / or, the sintering temperature is 330-360°C.
7. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: In the step b, the lubricating oil includes at least one of isoparaffin, naphtha, silicone oil and liquid paraffin; And / or, the particle size of the PTFE resin powder is 400-600nm.
8. The method for preparing a polytetrafluoroethylene microporous membrane according to claim 1, characterized in that: In the step b, the mass of the lubricating oil is 20-30% of the mass of the PTFE resin powder; And / or, the mass of the fluorocarbon hybrid surfactant is 0.5-3% of the mass of the PTFE resin powder.
9. A polytetrafluoroethylene microporous membrane, characterized in that: The method according to any one of claims 1 to 8 is adopted to prepare the present invention.
10. A proton exchange membrane, characterized in that: The invention comprises a polytetrafluoroethylene microporous membrane prepared by the method according to any one of claims 1 to 8 or a polytetrafluoroethylene microporous membrane according to claim 9.