Fast curing PE resin and preparation method thereof

A fast-curing PE resin is developed by modifying talcum powder and using zinc stearate, along with specific ratios of initiators and plasticizers, addressing the slow curing issue of traditional PE resin and enhancing mechanical and thermal properties for aerospace use.

CN119081266AInactive Publication Date: 2024-12-06GUANGDONG CHENBAO COMPOSITE MATERIAL CO LTD

Patent Information

Application Number
CN202411382240.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional PE resin curing speed is slow, limiting its application in the aerospace field where faster curing is required to enhance manufacturing efficiency.

Method used

A fast-curing PE resin is formulated using modified talcum powder, zinc stearate, and specific ratios of initiators and plasticizers, along with maleic anhydride grafted polyethylene, to improve compatibility and dispersibility, reducing curing time and enhancing mechanical properties.

Benefits of technology

The modified PE resin achieves significantly reduced curing time, improved mechanical strength, and enhanced thermal stability, making it suitable for aerospace applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005070183120000061
    Figure BDA0005070183120000061
  • Figure BDA0005070183120000071
    Figure BDA0005070183120000071
Patent Text Reader

Abstract

The invention discloses a fast curing PE resin and a preparation method thereof, and relates to the field of PE resin, and the fast curing PE resin comprises the following raw materials by weight: 40-80 parts of PE resin; 5-10 parts of an initiator; 5-15 parts of a cross-linking agent; 3-9 parts of a plasticizer; 2-6 parts of a stabilizer; 10 to 20 parts of zinc stearate; 15 to 35 parts of modified talcum powder; the modified talcum powder is prepared from the following raw materials: talcum powder, poly dimethyl diallyl ammonium chloride, KH560 and sodium dihydrogen phosphate. The method has the effect of prolonging the curing time of the PE resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of PE resins, in particular to a fast-curing PE resin and a preparation method thereof. Background Art

[0002] PE resin is a widely used thermoplastic with good chemical stability and electrical properties. The aerospace field has high requirements on the curing speed of materials. Fast-curing PE resin can be cured in a shorter time, thereby shortening the manufacturing cycle and improving production efficiency.

[0003] However, traditional PE resin has a slow curing speed, which limits its application in the aerospace field. Summary of the invention

[0004] In order to increase the curing speed of PE resin, the present application provides a fast-curing PE resin and a preparation method thereof.

[0005] In the first aspect, the present application provides a fast curing PE resin using the following technical solution: A fast-curing PE resin comprises the following raw materials in parts by weight: 40-80 parts of PE resin; 5-10 parts of initiator; 5-15 parts of crosslinking agent; 3-9 parts of plasticizer; 2-6 parts of stabilizer; 10-20 parts of zinc stearate; and 15-35 parts of modified talcum powder. The modified talcum powder is prepared from the following raw materials: talcum powder, polydimethyldiallylammonium chloride, KH560 and sodium dihydrogen phosphate.

[0006] By adopting the above technical scheme, PE resin is used as the resin matrix, and the present application modifies talcum powder, and the modified talcum powder is dispersed in the PE resin to improve the surface properties of the PE resin. Zinc stearate is used as a lubricant to reduce the friction of the PE resin during processing, improve processing efficiency, and help reduce the curing time of the PE resin. In the preparation process of the modified talcum powder, the mixed use of talcum powder, polydimethyldiallylammonium chloride, KH560 and sodium dihydrogen phosphate can improve the surface activity of talcum powder and its compatibility with the resin, thereby further improving the performance of composite materials of PE resin used in the aerospace field.

[0007] Preferably, the preparation method of the modified talc powder is: 5-15 parts by weight of talc powder and 10-20 parts by weight of polydimethyldiallylammonium chloride are mixed and stirred, and then 2-6 parts by weight of KH560 and 2-8 parts by weight of sodium dihydrogen phosphate are added and stirred continuously, and then the mixture is washed after centrifugation, dried, and ground to obtain the modified talc powder.

[0008] By adopting the above technical scheme, the present application modifies talcum powder, loads polydimethyldiallylammonium chloride on the surface of talcum powder, and cooperates with sodium dihydrogen phosphate to enhance the compatibility and dispersibility of talcum powder and PE resin, and KH560 reacts with hydroxyl groups on the surface of talcum powder to form chemical bonds, thereby improving the interfacial bonding force between talcum powder and PE resin, thereby enhancing the mechanical properties of PE resin.

[0009] Preferably, the particle size of the modified talc powder is in the range of 150-250 mesh.

[0010] By adopting the above technical solution and selecting a suitable particle size range of talc powder, the talc powder can be evenly dispersed in the PE resin, thereby improving the mechanical properties and thermal stability of the PE resin.

[0011] Preferably, the weight ratio of the talc powder, polydimethyldiallylammonium chloride and sodium dihydrogen phosphate is 1:(1.6-1.8):(0.3-0.4).

[0012] By adopting the above technical scheme, when talcum powder, polydimethyldiallyl ammonium chloride and sodium dihydrogen phosphate are in a specific weight ratio, polydimethyldiallyl ammonium chloride forms a uniform covering layer on the surface of talcum powder, and cooperates with sodium dihydrogen phosphate to help improve the dispersibility and compatibility of talcum powder and PE resin, reduce agglomeration, thereby enhancing the interface bonding force between modified talcum powder and PE resin, and improving the tensile strength of PE resin.

[0013] Preferably, the PE resin is a modified PE resin, and the preparation method of the modified PE resin is: 10-20 parts by weight of pearl powder is crushed and sieved, then calcined at high temperature, cooled, mixed with 10-15 parts by weight of maleic anhydride grafted polyethylene and 20-40 parts by weight of PE resin, and then melt-kneaded to obtain the modified PE resin.

[0014] By adopting the above technical solution, a fine pore structure appears on the surface of the pearl powder after high-temperature calcination, which can be evenly filled in the PE resin to improve the tensile strength of the PE resin. Maleic anhydride grafted polyethylene can effectively improve the compatibility between the pearl powder and the PE resin, making the PE resin structure tighter, thereby accelerating the curing time of the PE resin.

[0015] Preferably, the weight ratio of the pearl powder, maleic anhydride grafted polyethylene and PE resin is (0.4-0.5):(0.39-0.44):1.

[0016] By adopting the above technical scheme, when pearl powder, maleic anhydride grafted polyethylene and PE resin are in a specific weight ratio, the three work together to improve the mechanical properties and thermal stability of PE resin. Maleic anhydride grafted polypropylene reduces the melt viscosity of PE resin, which can improve the compatibility between PE resin and pearl powder. Pearl powder is dispersed in PE resin as an inorganic filler, which effectively improves the mechanical properties of PE resin.

[0017] Preferably, the weight ratio of the modified PE resin, zinc stearate and modified talc is (2.56-2.88):(0.48-0.6):1.

[0018] By adopting the above technical scheme, when the modified PE resin, zinc stearate and modified talc are in a specific weight ratio, the three cooperate together, the zinc stearate acts as a lubricant to reduce the melt viscosity of the PE resin, and the modified talc forms a protective layer in the PE resin matrix, promoting the modified talc to be evenly dispersed in the PE resin; at the same time, after the PE resin is modified, the wear on the surface of the PE resin is effectively reduced, and the thermal stability and mechanical strength of the PE resin are greatly improved.

[0019] Preferably, the initiator includes one of azobisisobutyronitrile and azobisisoheptanenitrile.

[0020] Preferably, the plasticizer includes one of dioctyl phthalate and dibutyl phthalate.

[0021] By adopting the above technical solution, selecting suitable initiators and plasticizers can help improve the processing properties of PE resin and significantly increase the curing speed of PE resin.

[0022] In the second aspect, the present application provides a method for preparing a fast-curing PE resin using the following technical solution: A method for preparing a fast-curing PE resin: comprising the following steps: heating and stirring the PE resin and modified talcum powder, adding an initiator, a cross-linking agent, a plasticizer, a stabilizer and zinc stearate and continuing to stir, granulating, cooling and cutting to obtain the fast-curing PE resin.

[0023] By adopting the above technical solution, PE resin is used as a matrix, each component is simply mixed with the PE resin according to steps, and PE resin with a short curing time can be obtained after granulation.

[0024] In summary, this application has the following beneficial technical effects: 1. PE resin is used as the resin matrix. The present application modifies talcum powder, and the modified talcum powder is dispersed in the PE resin to improve the surface properties of the PE resin. Zinc stearate is used as a lubricant to reduce the friction of the PE resin during processing, improve processing efficiency, and help reduce the curing time of the PE resin. In the preparation process of the modified talcum powder, the mixed use of talcum powder, polydimethyldiallylammonium chloride, KH560 and sodium dihydrogen phosphate can improve the surface activity of talcum powder and its compatibility with the resin, thereby further improving the performance of the composite material.

[0025] 2. The present application modifies talc powder by loading polydimethyldiallylammonium chloride on the surface of talc powder and cooperating with sodium dihydrogen phosphate to enhance the compatibility and dispersibility of talc powder and PE resin. KH560 reacts with hydroxyl groups on the surface of talc powder to form chemical bonds, thereby improving the interfacial bonding force between talc powder and PE resin, thereby enhancing the mechanical properties of PE resin. DETAILED DESCRIPTION

[0026] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example

[0027] Example 1 The present invention provides a method for preparing a fast-curing PE resin, comprising the following steps: 40g PE resin and 15g modified talc were heated and stirred at 80℃ and 300r / min for 10min, then 5g initiator, 5g crosslinker, 3g plasticizer, 2g stabilizer and 10g zinc stearate were added and stirred continuously, and then put into a twin-screw extruder and extruded and granulated at 180℃, and then cut after cooling to room temperature to obtain fast curing PE resin. The initiator is azobisisobutyronitrile, the crosslinker is diisopropyl peroxide, the plasticizer is dibutyl phthalate, the stabilizer is DOTTG, and the PE resin is selected from Dow 41E755 PE base material from the United States.

[0028] The preparation method of modified talcum powder is as follows: 5g talcum powder and 10g polydimethyldiallyl ammonium chloride are mixed and stirred at a temperature of 50°C for 2h, and then 2g KH560 and 2g sodium dihydrogen phosphate are added and stirred for 15min, and then centrifuged at a centrifugal speed of 10000r / min for 10min, washed with deionized water, dried at 60°C for 24h, and ground through 200 mesh to obtain modified talcum powder. Polydimethyldiallyl ammonium chloride is available from Hongzhuang Chemical Technology Co., Ltd., model number 26062-79-3.

[0029] Example 2 A method for preparing a fast-curing PE resin comprises the following steps: heating and stirring 80g of PE resin and 35g of modified talc at a temperature of 80°C and a rotation speed of 300r / min for 10min, adding 10g of initiator, 15g of cross-linking agent, 9g of plasticizer, 6g of stabilizer and 20g of zinc stearate and continuing stirring, putting into a twin-screw extruder, extruding and granulating at a temperature of 180°C, cooling to room temperature and cutting to obtain a fast-curing PE resin. The initiator is azobisisoheptanenitrile, the cross-linking agent is diisopropyl peroxide, the plasticizer is dioctyl phthalate, the stabilizer is DOTTG, and the PE resin is purchased from Dow 41E755PE base material of the United States.

[0030] The preparation method of modified talcum powder is as follows: 5g talcum powder and 10g polydimethyldiallyl ammonium chloride are mixed and stirred at a temperature of 50°C for 2h, and then 2g KH560 and 2g sodium dihydrogen phosphate are added and stirred for 15min, and then centrifuged at a centrifugal speed of 10000r / min for 10min, washed with deionized water, dried at 60°C for 24h, and ground through 200 mesh to obtain modified talcum powder. Polydimethyldiallyl ammonium chloride is available from Hongzhuang Chemical Technology Co., Ltd., model number 26062-79-3.

[0031] Example 3 A method for preparing a fast-curing PE resin comprises the following steps: heating and stirring PE resin and modified talcum powder at a temperature of 80°C and a rotation speed of 300r / min for 10 minutes, adding an initiator, a crosslinking agent, a plasticizer, a stabilizer and zinc stearate and continuing to stir, putting the mixture into a twin-screw extruder, extruding and granulating the mixture at a temperature of 180°C, and cutting the mixture after cooling to room temperature to obtain a fast-curing PE resin. The initiator is azobisisobutyronitrile, the crosslinking agent is diisopropyl peroxide, the plasticizer is dioctyl phthalate, the stabilizer is DOTTG, and the PE resin is selected from Dow 41E755 PE substrate of the United States.

[0032] The preparation method of modified talcum powder is as follows: 5g talcum powder and 10g polydimethyldiallyl ammonium chloride are mixed and stirred at a temperature of 50°C for 2h, and then 2g KH560 and 2g sodium dihydrogen phosphate are added and stirred for 15min, and then centrifuged at a centrifugal speed of 10000r / min for 10min, washed with deionized water, dried at 60°C for 24h, and ground through 200 mesh to obtain modified talcum powder. Polydimethyldiallyl ammonium chloride is available from Hongzhuang Chemical Technology Co., Ltd., model number 26062-79-3.

[0033] Example 4 A method for preparing a fast-curing PE resin, which is different from Example 3 in that, in the process of preparing modified talcum powder: 15g of talcum powder and 20g of polydimethyldiallyl ammonium chloride are mixed and stirred at a temperature of 50°C for 2h, and then 6g of KH560 and 8g of sodium dihydrogen phosphate are added and stirred for 15min, and then centrifuged at a centrifugal speed of 10000r / min for 10min, washed with deionized water, dried at 60°C for 24h, and ground through 200 mesh to obtain modified talcum powder. Polydimethyldiallyl ammonium chloride is purchased from Hongzhuang Chemical Technology Co., Ltd., model number 26062-79-3.

[0034] Example 5 A method for preparing a fast-curing PE resin, which is different from Example 3 in that: the input amount of talc is 10g, the input amount of polydimethyldiallylammonium chloride is 16g, and the input amount of sodium dihydrogen phosphate is 3g.

[0035] Example 6 A method for preparing a fast-curing PE resin, which is different from Example 3 in that: the input amount of talc is 10g, the input amount of polydimethyldiallylammonium chloride is 18g, and the input amount of sodium dihydrogen phosphate is 4g.

[0036] Example 7 A method for preparing a fast-curing PE resin, which is different from Example 6 in that an equal amount of PE resin is replaced with a modified PE resin, and the method for preparing the modified PE resin is as follows: 10g of pearl powder is crushed through a 150-mesh sieve, and then calcined at 1100°C for 2h in a box-type calcining furnace, and then cooled to room temperature, mixed with 10g of maleic anhydride grafted polyethylene and 20g of PE resin at a speed of 120r / min for 5min, and then melt-kneaded to obtain a modified PE resin. The maleic anhydride grafted polyethylene is purchased from Arkema, France, and the brand is 18410P.

[0037] Example 8 A method for preparing a fast-curing PE resin, which is different from Example 6 in that an equal amount of PE resin is replaced with a modified PE resin, and the method for preparing the modified PE resin is as follows: 20g of pearl powder is crushed through a 150-mesh sieve, and then calcined at 1100°C for 2h in a box-type calcining furnace, and then cooled to room temperature, mixed with 15g of maleic anhydride grafted polyethylene and 40g of PE resin at a speed of 120r / min for 5min, and then melt-kneaded to obtain a modified PE resin. The maleic anhydride grafted polyethylene is purchased from Arkema, France, and the brand is 18410P.

[0038] Example 9 A method for preparing a fast-curing PE resin, which is different from Example 8 in that: in the process of preparing the modified PE resin, the input amount of pearl powder is 12g, the input amount of maleic anhydride grafted polyethylene is 11.7g, and the input amount of PE resin is 30g.

[0039] Example 10 A method for preparing a fast-curing PE resin is different from Example 8 in that: in the process of preparing the modified PE resin, the input amount of pearl powder is 15g, the input amount of maleic anhydride grafted polyethylene is 13.2g, and the input amount of PE resin is 30g.

[0040] Embodiment 11 A method for preparing a fast-curing PE resin, which is different from Example 10 in that the input amount of the modified PE resin is 64 g, the input amount of zinc stearate is 12 g, and the input amount of the modified talc is 25 g.

[0041] Example 12 A method for preparing a fast-curing PE resin, which is different from Example 10 in that the input amount of the modified PE resin is 72 g, the input amount of zinc stearate is 15 g, and the input amount of the modified talc is 25 g.

[0042] Comparative Example Comparative Example 1 A method for preparing a fast-curing PE resin, which is different from Example 3 in that an equal amount of modified talcum powder is replaced with talcum powder.

[0043] Comparative Example 2 A method for preparing a fast-curing PE resin, which is different from Example 3 in that an equal amount of modified talc is replaced by calcium carbonate.

[0044] Comparative Example 3 A method for preparing a fast-curing PE resin, which is different from Example 3 in that an equal amount of calcium stearate is replaced with modified talc.

[0045] Comparative Example 4 A method for preparing a fast-curing PE resin, which is different from Example 3 in that: an equal amount of modified talc is replaced by modified calcium carbonate, wherein the modified calcium carbonate is prepared by mixing 5g of calcium carbonate and 10g of polydimethyldiallylammonium chloride at a temperature of 50°C and stirring for 2h, then adding 2g of KH560 and 2g of sodium dihydrogen phosphate and continuing to stir for 15min, centrifuging at a centrifugal speed of 10000r / min for 10min, washing with deionized water, drying at 60°C for 24h, and grinding through 200 mesh to obtain the modified calcium carbonate.

[0046] Performance testing: Curing time: The curing time of the PE resins prepared in Examples 1-12 and Comparative Examples 1-4 was tested according to the method for determining the gel time of unsaturated resins in GB 7193.6-1987.

[0047] Tensile strength test: The tensile strength of the PE resins prepared in Examples 1-12 and Comparative Examples 1-4 was tested according to the method of tensile properties of plastics in GB / T10401-2018.

[0048] Heat aging test: The PE resins prepared in Examples 1-12 and Comparative Examples 1-4 were aged in a heat aging box at 80° C. for 80 hours, and their tensile strength after aging was tested.

[0049] According to the data comparison of Examples 1-4 and Comparative Examples 1-4, PE resin is used as a resin matrix, and the present application modifies talcum powder, and the modified talcum powder is dispersed in the PE resin to improve the surface properties of the PE resin. Zinc stearate is used as a lubricant to reduce the friction of the PE resin during processing, improve processing efficiency, and help reduce the curing time of the PE resin. In the preparation process of the modified talcum powder, the mixed use of talcum powder, polydimethyldiallylammonium chloride, KH560 and sodium dihydrogen phosphate can improve the surface activity of talcum powder and its compatibility with the resin, thereby further improving the performance of the composite material.

[0050] According to the data comparison of Examples 3-6, when talcum powder, polydimethyldiallyl ammonium chloride and sodium dihydrogen phosphate are in a specific weight ratio, polydimethyldiallyl ammonium chloride forms a uniform covering on the surface of talcum powder, which, together with sodium dihydrogen phosphate, helps to improve the dispersibility and compatibility of talcum powder and PE resin, reduce agglomeration, thereby enhancing the interfacial bonding force between modified talcum powder and PE resin, and improving the tensile strength of PE resin.

[0051] According to the data comparison of Examples 6-8, after high-temperature calcination, the pearl powder has a fine pore structure on its surface, which can be evenly filled in the PE resin to improve the tensile strength of the PE resin. Maleic anhydride grafted polyethylene can effectively improve the compatibility between the pearl powder and the PE resin, making the PE resin structure more compact, thereby accelerating the curing time of the PE resin.

[0052] According to the data comparison of Examples 8-10, it can be obtained that when pearl powder, maleic anhydride grafted polyethylene and PE resin are in a specific weight ratio, the three work together to improve the mechanical properties and thermal stability of the PE resin. Maleic anhydride grafted polypropylene reduces the melt viscosity of the PE resin and can improve the compatibility between the PE resin and the pearl powder. The pearl powder is dispersed in the PE resin as an inorganic filler, which effectively improves the mechanical properties of the PE resin.

[0053] According to the data comparison of Examples 10-12, when the modified PE resin, zinc stearate and modified talc are in a specific weight ratio, the three cooperate together, zinc stearate acts as a lubricant to reduce the melt viscosity of the PE resin, and the modified talc forms a protective layer in the PE resin matrix, promoting the modified talc to be uniformly dispersed in the PE resin; at the same time, the modification of the PE resin effectively reduces the wear on the surface of the PE resin, greatly improving the thermal stability and mechanical strength of the PE resin.

[0054] The embodiments of the present application are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.

Claims

1. A fast curing PE resin, characterized in that: The invention comprises the following raw materials in parts by weight: 40-80 parts of PE resin, 5-10 parts of initiator, 5-15 parts of crosslinking agent, 3-9 parts of plasticizer, 2-6 parts of stabilizer, 10-20 parts of zinc stearate and 15-35 parts of modified talcum powder; the modified talcum powder is prepared from the following raw materials: talcum powder, polydimethyldiallylammonium chloride, KH560 and sodium dihydrogen phosphate.

2. A fast curing PE resin according to claim 1, characterized in that: The preparation method of the modified talc powder comprises: mixing 5-15 parts by weight of talc powder and 10-20 parts by weight of polydimethyldiallylammonium chloride, adding 2-6 parts by weight of KH560 and 2-8 parts by weight of sodium dihydrogen phosphate, and continuing to stir, washing after centrifugation, drying, and grinding to obtain the modified talc powder.

3. A fast curing PE resin according to claim 2, characterized in that: The particle size of the modified talc powder is in the range of 150-250 meshes.

4. A fast curing PE resin according to claim 2, characterized in that: The weight ratio of the talc powder, polydimethyldiallylammonium chloride and sodium dihydrogen phosphate is 1: (1.6-1.8): (0.3-0.4).

5. A fast curing PE resin according to claim 1, characterized in that: The PE resin is a modified PE resin, and the preparation method of the modified PE resin is: 10-20 parts by weight of pearl powder is crushed and sieved, then calcined at high temperature, cooled, mixed with 10-15 parts by weight of maleic anhydride grafted polyethylene and 20-40 parts by weight of PE resin, and then melt-kneaded to obtain the modified PE resin.

6. A fast curing PE resin according to claim 5, characterized in that: The weight ratio of the pearl powder, maleic anhydride grafted polyethylene and PE resin is (0.4-0.5): (0.39-0.44):

1.

7. A fast curing PE resin according to claim 5, characterized in that: The weight ratio of the modified PE resin, zinc stearate and modified talc is (2.56-2.88): (0.48-0.6):

1.

8. A fast curing PE resin according to claim 1, characterized in that: The initiator includes one of azobisisobutyronitrile and azobisisoheptanenitrile.

9. A fast curing PE resin according to claim 1, characterized in that: The plasticizer includes one of dioctyl phthalate and dibutyl phthalate.

10. A method for preparing a fast curing PE resin, characterized in that: The method for preparing the fast-curing PE resin according to any one of claims 1 to 9 comprises the following steps: heating and stirring the PE resin and modified talcum powder, adding an initiator, a crosslinking agent, a plasticizer, a stabilizer and zinc stearate and continuing to stir, granulating, cooling and cutting to obtain the fast-curing PE resin.

Citation Information

Patent Citations

  • Nano imvite talcum powder rotantional moulding-gradecross-linked polyethylene composite material and preparation method thereof

    CN102061027A

  • Regenerated polyethylene composition and preparation method thereof

    CN106916361A

  • High-temperature resistant composite packaging film and preparation method thereof

    CN111333991A

  • Environment-friendly polymer plastic film and preparation method thereof

    CN114716752A

Cited By

  • Wire insulating shell and preparation method thereof

    CN117777589A