Preparation method and application of lignin nano-clay composite material

By using sulfonic acid groups in lignin and nanocils to combine with metal ion coordination reaction and electrostatic attraction, the lignin structure and nanocil dispersion are changed, and the aggregation and precipitation problems are solved, and the secondary utilization of materials is realized. Meets the performance requirements of rubber composite materials.

CN119081435APending Publication Date: 2024-12-06HANGSHI TECH DEV (HANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411184150.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art cannot improve the stability of composite materials through reaction of sulfonic acid groups with metal ions, prevent the aggregation and precipitation of lignin and nanocils, and cannot change the lignin performance through ion exchange, increase the dispersion and stability of nanocils, and The secondary utilization of organic solvents cannot be achieved, resulting in the application of lignin nanoclay composites in rubber composites that cannot meet performance requirements.

Method used

By adding sulfonic acid groups to lignin and nanocil and reacting with metal ion coordination, electrostatic attraction is used to change the lignin structure, increase the dispersion and stability of nanocil, and achieve the resource two-dimensional Used again.

Benefits of technology

Effectively prevent the aggregation and precipitation of lignin and nanocil, improve the partial performance of lignin, improve the dispersion and stability of nanocil, realize the reuse of materials, save resources, and meet the performance needs of rubber composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081435A_ABST
    Figure CN119081435A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a lignin nano-clay composite material, and relates to the technical field of rubber composites.The preparation method of the lignin nano-clay composite material comprises the steps that sufficient modified lignin and modified nano-clay are weighed according to the proportion and dried for 2 h in the constant-temperature environment of 110 DEG C, and the lignin nano-clay composite material is obtained; the preparation method comprises the following steps: mixing and stirring the modified lignin and the modified nano-clay, adding an adhesive and an additive into the mixture, continuously stirring, and after the reaction is completed, carrying out molding and curing treatment on the composite material to obtain the product lignin nano-clay composite material. The additives are sodium lignin sulfonate, a sulfonated melamine formaldehyde condensate, sulfonate of maleic anhydride polyoxyethylene and a starch water reducer. Through coordination reaction of metal ions and sulfonic acid groups and electrostatic attraction, the problems of aggregation and precipitation of lignin and nano-clay in the preparation process of the lignin nano-clay composite material are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber composite materials, in particular to a preparation method of a lignin nano-clay composite material and application thereof. Background Art

[0002] With the development of science and technology, a single material often cannot meet the performance requirements in many fields. The birth of composite materials, by combining and superimposing different materials to achieve the performance of one plus one greater than one, is used to meet the performance requirements of materials in various fields. Rubber composite materials are obtained by compounding rubber with other materials, combining the advantages of various materials, and improving the performance of the overall material. Lignin is a complex organic polymer with unique aromatic and aliphatic Julian structures and rich functional groups. With the improvement of environmental awareness and the increase in demand for renewable energy, lignin has broad application prospects in many fields. Nanoclay is modified on its surface by ion exchange technology and other means. Adding the modified nanoclay to the preparation of composite materials can significantly improve the mechanical properties, thermal stability and barrier properties of the composite materials. Rubber composites are based on the combination of rubber materials and other nano or micro fillers to improve the performance of rubber to meet the growing needs in different fields. The fillers are evenly distributed through different preparation processes such as solution blending, melt blending and intercalation compounding, so that the rubber composite has better mechanical properties, thermal stability, conductivity and other properties. Rubber composites with more characteristics have broad application prospects in many fields.

[0003] Patent document CN115521481B discloses a new type of anti-cutting resin, its preparation method and its application in the preparation of rubber composite materials. The above patent realizes that after the modified lignin is polymerized with dicyclopentadiene, a denser cross-linked network can be formed, thereby preventing the reduction of resin performance. The ring structure of the modified lignin is similar to the structure in rubber, which further enhances the compatibility. Lignin, as the matrix of this anti-cutting resin, has its own anti-aging, reinforcement and heat reduction properties, which also makes this new type of anti-cutting resin more widely used and cheaper, but the above patent cannot be realized.

[0004] Patent document CN112831059B discloses a modified lignin, a preparation method thereof and an application thereof in a rubber composite material. The above patent realizes that the structure of the acetylenic reagent contains an acyl chloride functional group, which is easy to undergo esterification reaction with the alcoholic hydroxyl group and the phenolic hydroxyl group in the lignin molecule to generate a modified lignin grafted with an unsaturated acetylenic functional group; the acetylenic modification reduces the hydroxyl content in the lignin molecule, reduces the molecular polarity, helps to inhibit the self-aggregation tendency of lignin caused by hydrogen bonds, is conducive to grinding to obtain a lignin powder with a smaller particle size, improves the compatibility and affinity of lignin with non-polar natural rubber, and promotes the dispersion of lignin in the natural rubber matrix, but the above patent cannot be achieved.

[0005] Patent document CN113583254B discloses a cross-linkable lignin and its preparation method and application in rubber composite materials. The above patent realizes that the acid anhydride contained in the prepared cross-linkable modifier reacts with the hydroxyl groups in the lignin molecules to reduce the polar hydroxyl content, generate lignin grafted with long-chain unsaturated olefins, reduce the polarity of lignin, improve the compatibility between lignin and natural rubber, and facilitate the dispersion of lignin in the rubber matrix, but the above patent cannot be achieved.

[0006] Patent document CN106905712B discloses a method for preparing rubber fillers by neutralizing alkali lignin with inorganic salts. The above patent achieves significant improvement in the mechanical properties of rubber composite materials prepared with rubber fillers, such as tensile strength, tensile stress, elongation at break and hardness, but the above patent cannot be achieved.

[0007] In summary, the above patents cannot achieve the improvement of the stability of the composite material by reacting the sulfonic acid group with the metal ions, preventing the aggregation and precipitation of lignin and nanoclay, changing the original properties of lignin by ion exchange, and significantly increasing some properties of lignin, and cannot achieve the modification of nanoclay during the processing of nanoclay, and increasing the dispersibility and stability of nanoclay by reorganizing the internal structure of nanoclay, and cannot achieve the secondary utilization of resources by dissolving the material with an organic solvent and separating and precipitating it, thereby improving the utilization rate of materials and saving resources. As a result, the lignin nanoclay composite material and its application in rubber composite materials cannot meet the performance requirements in the field of rubber composite material technology; To this end, the present application proposes a method for improving the stability of the composite material by reacting the sulfonic acid group with the metal ion, preventing the aggregation and precipitation of lignin and nanoclay, changing the original properties of lignin by ion exchange, greatly increasing some properties of lignin, modifying the nanoclay during the processing process, increasing the dispersibility and stability of the nanoclay by reorganizing the internal structure of the nanoclay, dissolving the material in an organic solvent and separating and precipitating it, performing secondary utilization of resources, improving material utilization, and saving resources. The preparation method of lignin nanoclay composite material and its application in rubber composite material are disclosed. Summary of the invention

[0008] The object of the present invention is to provide a preparation method and application of a lignin nanoclay composite material, so as to solve the technical problems proposed in the above-mentioned background technology that the stability of the composite material cannot be improved by reacting the sulfonic acid group with the metal ion, the aggregation and precipitation of lignin and nanoclay cannot be prevented, the original properties of lignin cannot be changed by ion exchange, and some properties of lignin cannot be greatly increased, the nanoclay cannot be modified during the processing process to increase the dispersibility and stability of the nanoclay by reorganizing the internal structure of the nanoclay, and the material cannot be dissolved by an organic solvent and then separated and precipitated for secondary utilization of resources, thereby improving material utilization and saving resources, resulting in that the lignin nanoclay composite material and its application in the rubber composite material cannot meet the performance requirements in the field of rubber composite material technology.

[0009] To achieve the above object, the present invention provides the following technical solution: a preparation of a lignin nanoclay composite material, the preparation steps of the lignin nanoclay composite material are: Step 1: Weigh sufficient amount of modified lignin and modified nanoclay according to proportion, and dry them in a constant temperature environment of 110°C for 2h; Step 2: Mixing and stirring the modified lignin and the modified nanoclay; Step 3: Add adhesive and additives to the mixture and continue stirring; Step 4: After the reaction is completed, the composite material is molded and cured to obtain a lignin nanoclay composite material; The additives are sodium lignin sulfonate, sulfonated melamine formaldehyde condensate, maleic anhydride polyoxyethylene sulfonate and starch water reducer.

[0010] Preferably, the sulfonic acid groups in the additive component react with the metal ions inside the lignin and nanoclay to form coordination bonds. At the same time, the hydrogen ions ionized from the sulfonic acid groups make the lignin molecules negatively charged, while the surface of the nanoclay has a certain charge. By adding the sulfonic acid groups, the lignin molecules and the nanoclay can be combined with each other through electrostatic attraction.

[0011] Preferably, the adhesive is a lignin-based adhesive, which is prepared using highly active lignin. Compared with traditional petrochemical-based adhesives that produce toxic gases during use, lignin-based adhesives are greener, low-carbon, environmentally friendly and sustainable.

[0012] Preferably, the lignin component comprises the following components in parts by weight: Wood blocks: 20 to 50 pieces; Organic solvent: 40 to 80 parts; Cationic solution: 10 to 40 parts; Acidifier: 5 to 10 parts; Sodium aminobenzenesulfonate: 1 to 5 parts; Distilled water: 10 to 15 parts; Acetone solution: 20 to 50 parts; Metaphenylenediamine: 1 to 5 parts; Methacrylic anhydride: 0.2 to 0.5 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.

[0013] Preferably, the preparation process of the lignin is: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: Modify the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtain modified lignin after filtering and drying.

[0014] Preferably, the preparation steps of the nanoclay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: Add water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: Separate, purify and dry the reaction mixture to obtain modified nanoclay.

[0015] Preferably, the modifier is composed of: dimethyl didecyl ammonium chloride, phthalate coupling agent, dodecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride and sodium dodecyl benzene sulfonate.

[0016] Preferably, the application steps of the lignin nanoclay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: The mixed material is subjected to hot pressing to obtain the final product, a rubber composite material.

[0017] Preferably, the weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1.

[0018] Preferably, the weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9.

[0019] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention is designed to prevent the aggregation and precipitation of lignin and nanoclay by the coordination reaction of the sulfonic acid group in the additive with the metal ions in the raw materials and electrostatic attraction during the preparation process of the lignin nanoclay composite material; 2. The present invention is designed to add a cationic solution during the preparation stage of lignin, and through ion exchange, the internal structure of lignin is changed, some properties of lignin are improved, and the application prospects of lignin are broadened; 3. The present invention is designed to add a modifier during the preparation process of nanoclay to reorganize the internal structure of nanoclay, thereby increasing the dispersibility and stability of nanoclay and improving the performance of the product; 4. The present invention is designed to dissolve the material with an organic solvent and then separate and precipitate it, thereby achieving the reuse of materials, saving resources, and being green and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a schematic diagram of the preparation process of modified lignin of the present invention; Figure 2 Schematic diagram of the preparation process of modified nanoclay of the present invention; Figure 3 This is a schematic diagram of the preparation process of the lignin nanoclay composite material of the present invention; Figure 4 This is a schematic diagram of the application of the lignin nano-clay composite material of the present invention in a rubber composite material; DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example

[0022] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 , a method for preparing a lignin nanoclay composite material, the preparation steps of the lignin nanoclay composite material are: Step 1: Weigh sufficient amount of modified lignin and modified nanoclay according to proportion, and dry them in a constant temperature environment of 110°C for 2h; Step 2: Mixing and stirring the modified lignin and the modified nanoclay; Step 3: Add adhesive and additives to the mixture and continue stirring Step 4: After the reaction is completed, the composite material is molded and cured to obtain a lignin nanoclay composite material; The additives are: sodium lignin sulfonate, sulfonated melamine formaldehyde condensate, maleic anhydride polyoxyethylene sulfonate and starch water reducer; The sulfonic acid groups in the additive component react with the metal ions inside the lignin and nanoclay to form coordination bonds. At the same time, the hydrogen ions ionized from the sulfonic acid groups make the lignin molecules negatively charged, while the surface of the nanoclay has a certain charge. By adding the sulfonic acid groups, the lignin molecules and the nanoclay can be combined with each other through electrostatic attraction. The adhesive is a lignin-based adhesive, which is prepared using highly active lignin. Compared with traditional petrochemical-based adhesives that produce toxic gases during use, lignin-based adhesives are greener, low-carbon, environmentally friendly and sustainable. The preparation of the lignin comprises the following components in parts by weight: Wood blocks: 40 pieces; Organic solvent: 50 parts; Cationic solution: 20 parts; Acidifier: 7 parts; Sodium aminobenzenesulfonate: 3 parts; Distilled water: 13 parts; Acetone solution: 22 parts; Metaphenylenediamine: 2 parts; Methacrylic anhydride: 0.2 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.; The preparation steps of the lignin are: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: modifying the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtaining modified lignin after filtering and drying; The preparation steps of the nanoclay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: Add water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: separating, purifying and drying the reaction mixture to obtain modified nanoclay; The modifier is composed of: silane, phthalate coupling agent, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and sodium dodecylbenzenesulfonate; The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: hot pressing the mixed material to obtain the final product, a rubber composite material; The weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; Further, 40 parts of wood blocks, 50 parts of organic solvents, 20 parts of cationic solutions, 7 parts of acidulants, 3 parts of sodium aminobenzenesulfonate, 10 parts of distilled water and 20 parts of acetone solutions were prepared, the wood blocks were crushed into powder, dried in an environment of 120° C. for 1.3 hours, the wood powder and the organic solvent were mixed and stirred, the cationic solution was added and continued to be stirred, distilled water heated to 70° C. was added to regenerate cellulose, the solution after cellulose regeneration was separated by centrifugation, the acetone solution was added to the separated mixed solution B to precipitate lignin, the lignin was acid-washed and dried, the modifier was added to the purified lignin, and modified lignin was obtained after filtering and drying; Prepare a sufficient amount of montmorillonite, crush it into powder, sieve and dry the montmorillonite powder, the size of the sieved montmorillonite powder is 350nm, the drying temperature is 30°C, the time is 3h, add the treated montmorillonite powder to a powder metallurgy sintering device and sinter at 600°C for 5h, perform ion exchange reaction on the sintered material, purify and dry the reacted material, add water to the material to form montmorillonite powder, add a modifier thereto, fully stir, filter and dry to obtain modified nano clay; The modified lignin and modified nanoclay are weighed in a weight ratio of 0.8:1, dried at 110°C for 2 hours, mixed and stirred, adhesives and additives are added during the process, the mixed material is molded and cured in a press to obtain a lignin nanoclay composite material, the lignin nanoclay composite material, carbon black and natural rubber are weighed according to a ratio, put into an internal mixer for mixing, a vulcanizing agent is added during the mixing process, and the mixture is hot-pressed to obtain the final product, a rubber composite material. Example

[0023] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 , a method for preparing a lignin nano-clay composite material, the preparation steps of the lignin nano-clay composite material are: Step 1: Weigh sufficient amount of modified lignin and modified nanoclay according to proportion, and dry them in a constant temperature environment of 110°C for 2h; Step 2: Mixing and stirring the modified lignin and the modified nanoclay; Step 3: Add adhesive and additives to the mixture and continue stirring Step 4: After the reaction is completed, the composite material is molded and cured to obtain a lignin nanoclay composite material; The additives are: sodium lignin sulfonate, sulfonated melamine formaldehyde condensate, maleic anhydride polyoxyethylene sulfonate and starch water reducer; The sulfonic acid groups in the additive component react with the metal ions inside the lignin and nanoclay to form coordination bonds. At the same time, the hydrogen ions ionized from the sulfonic acid groups make the lignin molecules negatively charged, while the surface of the nanoclay has a certain charge. By adding the sulfonic acid groups, the lignin molecules and the nanoclay can be combined with each other through electrostatic attraction. The adhesive is a lignin-based adhesive, which is prepared using highly active lignin. Compared with traditional petrochemical-based adhesives that produce toxic gases during use, lignin-based adhesives are greener, low-carbon, environmentally friendly and sustainable. The preparation of the lignin comprises the following components in parts by weight: Wood blocks: 40 pieces; Organic solvent: 50 parts; Cationic solution: 20 parts; Acidifier: 7 parts; Sodium aminobenzenesulfonate: 3 parts; Distilled water: 13 parts; Acetone solution: 22 parts; Metaphenylenediamine: 2 parts; Methacrylic anhydride: 0.2 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.; The preparation steps of the lignin are: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: modifying the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtaining modified lignin after filtering and drying; The preparation steps of the nanoclay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: Add water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: separating, purifying and drying the reaction mixture to obtain modified nanoclay; The modifier is composed of: silane, phthalate coupling agent, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and sodium dodecylbenzenesulfonate; The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: hot pressing the mixed material to obtain the final product, a rubber composite material; The weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; Further, 40 parts of wood blocks, 50 parts of organic solvents, 20 parts of cationic solutions, 7 parts of acidulants, 3 parts of sodium aminobenzenesulfonate, 10 parts of distilled water and 20 parts of acetone solutions were prepared, the wood blocks were crushed into powder, dried in an environment of 120° C. for 1.3 hours, the wood powder and the organic solvent were mixed and stirred, the cationic solution was added and continued to be stirred, distilled water heated to 70° C. was added to regenerate cellulose, the solution after cellulose regeneration was separated by centrifugation, the acetone solution was added to the separated mixed solution B to precipitate lignin, the lignin was acid-washed and dried, the modifier was added to the purified lignin, and modified lignin was obtained after filtering and drying; Prepare a sufficient amount of montmorillonite, crush it into powder, sieve and dry the montmorillonite powder, the size of the sieved montmorillonite powder is 350nm, the drying temperature is 30°C, the time is 3h, add the treated montmorillonite powder to a powder metallurgy sintering device and sinter at 600°C for 5h, perform ion exchange reaction on the sintered material, purify and dry the reacted material, add water to the material to form montmorillonite powder, add a modifier thereto, fully stir, filter and dry to obtain modified nano clay; The modified lignin and modified nanoclay are weighed in a weight ratio of 0.6:1, dried at 110°C for 2 hours, mixed and stirred, adhesives and additives are added during the process, the mixed material is molded and cured in a press to obtain a lignin nanoclay composite material, the lignin nanoclay composite material, carbon black and natural rubber are weighed according to a ratio, put into an internal mixer for mixing, a vulcanizing agent is added during the mixing process, and the mixture is hot-pressed to obtain the final product, a rubber composite material. Example

[0024] See also Figure 1 , Figure 2 , Figure 3 and Figure 4 , a method for preparing a lignin nanoclay composite material, the preparation steps of the lignin nanoclay composite material are: Step 1: Weigh sufficient amount of modified lignin and modified nanoclay according to proportion, and dry them in a constant temperature environment of 110°C for 2h; Step 2: Mixing and stirring the modified lignin and the modified nanoclay; Step 3: Add adhesive and additives to the mixture and continue stirring Step 4: After the reaction is completed, the composite material is molded and cured to obtain a lignin nanoclay composite material; The additives are: sodium lignin sulfonate, sulfonated melamine formaldehyde condensate, maleic anhydride polyoxyethylene sulfonate and starch water reducer; The sulfonic acid groups in the additive component react with the metal ions inside the lignin and nanoclay to form coordination bonds. At the same time, the hydrogen ions ionized from the sulfonic acid groups make the lignin molecules negatively charged, while the surface of the nanoclay has a certain charge. By adding the sulfonic acid groups, the lignin molecules and the nanoclay can be combined with each other through electrostatic attraction. The adhesive is a lignin-based adhesive, which is prepared using highly active lignin. Compared with traditional petrochemical-based adhesives that produce toxic gases during use, lignin-based adhesives are greener, low-carbon, environmentally friendly and sustainable. The preparation of the lignin comprises the following components in parts by weight: Wood blocks: 40 pieces; Organic solvent: 50 parts; Cationic solution: 20 parts; Acidifier: 7 parts; Sodium aminobenzenesulfonate: 3 parts; Distilled water: 13 parts; Acetone solution: 22 parts; Metaphenylenediamine: 2 parts; Methacrylic anhydride: 0.2 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.; The preparation steps of the lignin are: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: modifying the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtaining modified lignin after filtering and drying; The preparation steps of the nanoclay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: Add water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: separating, purifying and drying the reaction mixture to obtain modified nanoclay; The modifier is composed of: silane, phthalate coupling agent, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and sodium dodecylbenzenesulfonate; The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: hot pressing the mixed material to obtain the final product, a rubber composite material; The weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; Further, 40 parts of wood blocks, 50 parts of organic solvents, 20 parts of cationic solutions, 7 parts of acidulants, 3 parts of sodium aminobenzenesulfonate, 10 parts of distilled water and 20 parts of acetone solutions were prepared, the wood blocks were crushed into powder, dried in an environment of 120° C. for 1.3 hours, the wood powder and the organic solvent were mixed and stirred, the cationic solution was added and continued to be stirred, distilled water heated to 70° C. was added to regenerate cellulose, the solution after cellulose regeneration was separated by centrifugation, the acetone solution was added to the separated mixed solution B to precipitate lignin, the lignin was acid-washed and dried, the modifier was added to the purified lignin, and modified lignin was obtained after filtering and drying; Prepare a sufficient amount of montmorillonite, crush it into powder, sieve and dry the montmorillonite powder, the size of the sieved montmorillonite powder is 350nm, the drying temperature is 30°C, the time is 3h, add the treated montmorillonite powder to a powder metallurgy sintering device and sinter at 600°C for 5h, perform ion exchange reaction on the sintered material, purify and dry the reacted material, add water to the material to form montmorillonite powder, add a modifier thereto, fully stir, filter and dry to obtain modified nano clay; The modified lignin and modified nanoclay are weighed in a weight ratio of 1:1, dried at 110°C for 2 hours, mixed and stirred, adhesives and additives are added during the process, the mixed material is molded and cured in a press to obtain a lignin nanoclay composite material, the lignin nanoclay composite material, carbon black and natural rubber are weighed according to a ratio, put into an internal mixer for mixing, a vulcanizing agent is added during the mixing process, and the mixture is hot-pressed to obtain the final product, a rubber composite material. Example

[0025] See also Figure 1 and Figure 4 , a preparation method and application of a lignin nano-clay composite material, wherein the preparation of the lignin comprises the following components in parts by weight: Wood blocks: 40 pieces; Organic solvent: 50 parts; Cationic solution: 20 parts; Acidifier: 7 parts; Sodium aminobenzenesulfonate: 3 parts; Distilled water: 13 parts; Acetone solution: 22 parts; Metaphenylenediamine: 2 parts; Methacrylic anhydride: 0.2 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.; The preparation steps of the lignin are: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: modifying the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtaining modified lignin after filtering and drying; The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: hot pressing the mixed material to obtain the final product, a rubber composite material; The weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; Further, 40 parts of wood blocks, 50 parts of organic solvents, 20 parts of cationic solutions, 7 parts of acidulants, 3 parts of sodium aminobenzenesulfonate, 10 parts of distilled water and 20 parts of acetone solutions were prepared, the wood blocks were crushed into powder, dried in an environment of 120° C. for 1.3 hours, the wood powder and the organic solvent were mixed and stirred, the cationic solution was added and continued to be stirred, distilled water heated to 70° C. was added to regenerate cellulose, the solution after cellulose regeneration was separated by centrifugation, the acetone solution was added to the separated mixed solution B to precipitate lignin, the lignin was acid-washed and dried, the modifier was added to the purified lignin, and modified lignin was obtained after filtering and drying; The modified lignin, carbon black and natural rubber are weighed in a ratio of (0.5:0.7:1), put into an internal mixer for mixing, a vulcanizing agent is added during mixing, and the mixture is hot-pressed to obtain the final product, a rubber composite material. Example

[0026] See also Figure 2 and Figure 4 , a preparation method of a lignin nanoclay composite material and its application, the preparation steps of the nanoclay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: Add water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: separating, purifying and drying the reaction mixture to obtain modified nanoclay; The modifier is composed of: silane, phthalate coupling agent, dodecyltrimethylammonium chloride, hexadecyltrimethylammonium chloride and sodium dodecylbenzenesulfonate; The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: hot pressing the mixed material to obtain the final product, a rubber composite material; The weight ratio of the lignin nanoclay composite material to the natural rubber is 0.2-0.6:1; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; The weight ratio of the lignin nanoclay composite material to carbon black is 1:0.6-0.9; Further, 40 parts of wood blocks, 50 parts of organic solvents, 20 parts of cationic solutions, 7 parts of acidulants, 3 parts of sodium aminobenzenesulfonate, 10 parts of distilled water and 20 parts of acetone solutions were prepared, the wood blocks were crushed into powder, dried in an environment of 120° C. for 1.3 hours, the wood powder and the organic solvent were mixed and stirred, the cationic solution was added and continued to be stirred, distilled water heated to 70° C. was added to regenerate cellulose, the solution after cellulose regeneration was separated by centrifugation, the acetone solution was added to the separated mixed solution B to precipitate lignin, the lignin was acid-washed and dried, the modifier was added to the purified lignin, and modified lignin was obtained after filtering and drying; Prepare a sufficient amount of montmorillonite, crush it into powder, sieve and dry the montmorillonite powder, the size of the sieved montmorillonite powder is 350nm, the drying temperature is 30°C, the time is 3h, add the treated montmorillonite powder to a powder metallurgy sintering device and sinter at 600°C for 5h, perform ion exchange reaction on the sintered material, purify and dry the reacted material, add water to the material to form montmorillonite powder, add a modifier thereto, fully stir, filter and dry to obtain modified nano clay; The modified nano clay, carbon black and natural rubber are weighed in a ratio of (0.5:0.7:1), put into an internal mixer for mixing, a vulcanizing agent is added during mixing, and the mixture is hot-pressed to obtain the final product, a rubber composite material.

[0027] Performance Testing The rubber composite materials of Examples 1-5 were subjected to performance testing, with reference to GB / T528-2009, and tested in a CMT6503 rubber electronic universal testing machine.

[0028]

[0029] Working principle: prepare 20 to 50 parts of wood blocks, 40 to 80 parts of organic solvents, 10 to 40 parts of cationic solutions, 5 to 10 parts of acidifiers, 1 to 5 parts of sodium aminobenzenesulfonate, 10 to 15 parts of distilled water, 20 to 50 parts of acetone solutions, 1 to 5 parts of metaphenylenediamine and 0.2 to 0.5 parts of methacrylic anhydride, crush the wood blocks into powder, dry them in an environment of 120°C for 1.3 hours, mix the wood powder and the organic solvent, add the cationic solution and continue to stir, add distilled water heated to 70°C to regenerate cellulose, separate the solution after cellulose regeneration by centrifugation, add acetone solution to the separated mixed solution B to precipitate lignin, acid wash and dry the lignin, add sodium aminobenzenesulfonate, metaphenylenediamine and methacrylic anhydride to the purified lignin, and obtain modified lignin after filtering and drying; Prepare a sufficient amount of montmorillonite, crush it into powder, sieve and dry the montmorillonite powder, the size of the sieved montmorillonite powder is 350nm, the drying temperature is 30°C, the time is 3h, add the treated montmorillonite powder to a powder metallurgy sintering device and sinter at 600°C for 5h, perform ion exchange reaction on the sintered material, purify and dry the reacted material, add water to the material to form montmorillonite powder, add a modifier thereto, fully stir, filter and dry to obtain modified nano clay; The modified lignin and modified nanoclay are weighed in a weight ratio of 0.8:1, dried at 110°C for 2 hours, mixed and stirred, adhesives and additives are added during the process, the mixed material is molded and cured in a press to obtain a lignin nanoclay composite material, the lignin nanoclay composite material, carbon black and natural rubber are weighed according to a ratio, put into an internal mixer for mixing, a vulcanizing agent is added during the mixing process, and the mixture is hot-pressed to obtain the final product, a rubber composite material.

[0030] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a lignin nanoclay composite material, characterized in that: The preparation steps of lignin nanoclay composite material are: Step 1: Weigh sufficient amount of modified lignin and modified nanoclay according to proportion, and dry them in a constant temperature environment of 110°C for 2h; Step 2: Mixing and stirring the modified lignin and the modified nanoclay; Step 3: Add adhesive and additives to the mixture and continue stirring; Step 4: After the reaction is completed, the composite material is molded and cured to obtain a lignin nanoclay composite material; The additives are sodium lignin sulfonate, sulfonated melamine formaldehyde condensate, maleic anhydride polyoxyethylene sulfonate and starch water reducer.

2. The method for preparing a lignin nanoclay composite material according to claim 1, characterized in that: The sulfonic acid groups in the additive component react with the metal ions inside the lignin and nanoclay to form coordination bonds. At the same time, the hydrogen ions ionized from the sulfonic acid groups make the lignin molecules negatively charged, while the surface of the nanoclay has a certain charge. By adding the sulfonic acid groups, the lignin molecules and the nanoclay can be combined with each other through electrostatic attraction.

3. The method for preparing a lignin nanoclay composite material according to claim 1, characterized in that: The adhesive is a lignin-based adhesive, which is prepared using highly active lignin. Compared with traditional petrochemical-based adhesives that produce toxic gases during use, lignin-based adhesives are greener, low-carbon, environmentally friendly and sustainable.

4. The method for preparing a lignin nanoclay composite material according to claim 1, characterized in that: The lignin component includes the following components in parts by weight: Wood blocks: 20 to 50 pieces; Organic solvent: 40 to 80 parts; Cationic solution: 10 to 40 parts; Acidifier: 5 to 10 parts; Sodium aminobenzenesulfonate: 1 to 5 parts; Distilled water: 10 to 15 parts; Acetone solution: 20 to 50 parts; Metaphenylenediamine: 1 to 5 parts; Methacrylic anhydride: 0.2 to 0.5 parts; The components of the organic solvent are: dioxane, toluene, 1,2-dichloroethane and ethanol; The cationic solution contains: sodium ions, potassium ions, ammonium ions, silver ions and zinc ions, etc.

5. The method for preparing a lignin nanoclay composite material according to claim 1, characterized in that: The preparation process of the lignin is as follows: Step 1: Prepare enough wood blocks, chop and grind them into wood powder and set aside; Step 2: Mix the wood powder and the organic solvent, add the cationic solution, and stir thoroughly; Step 3: adding heated distilled water to the mixed solution A to regenerate cellulose; Step 4: filtering and separating the liquid after cellulose regeneration, and distilling the filtrate to separate the organic solvent, water and mixed solution B; Step 5: adding a sufficient amount of acetone solution to the mixed solution B to precipitate lignin; Step 6: After acid washing and drying the precipitated lignin, lignin is obtained; Step 7: Modify the purified lignin by adding sodium aminobenzenesulfonate, m-phenylenediamine and methacrylic anhydride to the lignin, and obtain modified lignin after filtering and drying.

6. The method for preparing a lignin nanoclay composite material according to claim 1, characterized in that: The preparation steps of the nano clay are: Step 1: Prepare enough montmorillonite and crush it into powder; Step 2: pre-treating montmorillonite powder; Step 3: sintering the pretreated montmorillonite powder at 600°C; Step 4: Perform ion exchange reaction on the sintered material while continuing to fully stir the material; Step 5: Purify the material and dry the purified material; Step 6: adding water to the purified material to form montmorillonite powder; Step 7: Add the modifier to the montmorillonite powder and stir thoroughly at a constant temperature of 60°C; Step 7: Separate, purify and dry the reaction mixture to obtain modified nanoclay.

7. The method for preparing a lignin nanoclay composite material according to claim 6, characterized in that: The modifier comprises: dimethyl didecyl ammonium chloride, phthalate coupling agent, dodecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride and sodium dodecyl benzene sulfonate.

8. An application of a lignin nano-clay composite material in a rubber composite material, applicable to a preparation method of a lignin nano-clay composite material according to any one of claims 1 to 7, characterized in that: The application steps of the lignin nano-clay composite material in the rubber material are: Step 1: Prepare sufficient amounts of lignin nanoclay composite material, carbon black, and natural rubber; Step 2: putting the lignin nanocomposite material, carbon black and natural rubber into an internal mixer for mixing; Step 3: Adding vulcanizing agent during mixing; Step 4: The mixed material is subjected to hot pressing to obtain the final product, a rubber composite material.

9. The use of a lignin nanoclay composite material in a rubber composite material according to claim 8, characterized in that: The weight ratio of the lignin nano-clay composite material to the natural rubber is 0.2-0.6:

1.