Water-based high-temperature-resistant epoxy static conductive coating as well as preparation method and application thereof
By using aqueous phenolic epoxy emulsions, epoxy modified silicone emulsions and single-wall carbon nanotubes in aqueous epoxy electrostatic coatings, the poor coating performance and the threat of active metal anti-rust pigments to catalysts under high temperature environments are solved. The problem is that the high temperature resistance and corrosion resistance of high-temperature storage tanks have been improved.
Patent Information
- Application Number
- CN202411171250.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-06
AI Technical Summary
The existing water-based epoxy electrostatic coatings have poor performance in high temperature environments, and the use of active metal anti-rust pigments poses a threat to the catalyst, affecting the safety and efficiency of storage tank equipment.
The aqueous phenolic epoxy emulsion is used in combination with the aqueous epoxy modified silicone emulsion, and the aqueous single-wall carbon nanotubes are used as the conductive agent to avoid the use of anti-rust pigments, and the high temperature resistance and electrostatic conductivity of the coating are improved through specific formulations.
The coating has achieved good high temperature resistance and corrosion resistance under an environment above 120°C, and its stability is improved, which avoids the coating discoloration and rust problems, and reduces the toxicity effect on the catalyst.
Smart Images

Figure BDA0005009335340000071 
Figure BDA0005009335340000081 
Figure BDA0005009335340000082
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and particularly relates to a water-based high-temperature-resistant epoxy static-conductive coating and a preparation method and application thereof. Background Art
[0002] Chinese patent CN115286976A discloses a long-term protective water-based phenolic epoxy electrostatic conductive coating and a preparation method thereof, and introduces a long-term protective electrostatic conductive coating prepared by cold-mixing water-based phenolic epoxy emulsion with water-based epoxy-modified acrylic emulsion. The coating has the technical advantages of low VOCs (volatile organic compounds), high electrostatic conductive stability, excellent adhesion, water resistance, boiling resistance, chemical resistance, good weather resistance, and excellent anti-corrosion performance. However, active metal anti-rust pigments are added to the formula, and these metal elements will have an adverse effect on the oil products carried. For example, in the catalytic cracking process of light oil, fuel oil, etc., the metal elements poison the catalyst, threaten the safety of the equipment and reduce the catalytic efficiency.
[0003] Chinese patent CN115820075A discloses a water-based static conductive coating for storage tanks and its preparation method, introducing a method of using a water-based solid epoxy emulsion and a water-based phenolic epoxy emulsion, using inert fillers and conductive mica powder and galvanized glass microspheres less than 1 micron, to prepare a water-based static conductive coating for storage tanks, which improves hot water resistance, slows penetration speed, and improves corrosion resistance. The coating does not consider the high temperature resistance of the coating coating, and uses a lot of mica powder as filler, resulting in high viscosity of the paint and poor construction convenience.
[0004] The above schemes all provide water-based epoxy antistatic coatings for room temperature storage tanks, whose conductivity and corrosion resistance can meet the requirements of petrochemical storage tanks, but none of them examines the performance of epoxy antistatic coatings for storage tanks at high temperatures.
[0005] Therefore, there is an urgent need to provide a new coating that not only has good static conductivity and anti-corrosion properties, but also has high temperature resistance. Summary of the invention
[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a water-based high temperature resistant epoxy electrostatic conductive coating and its preparation method and application. The coating of the present invention not only has good electrostatic conductive and anti-corrosion properties, but also has high temperature resistance, and is very suitable for chemical equipment, especially high temperature resistant chemical equipment (such as petrochemical storage tanks) as electrostatic conductive and anti-corrosion coatings.
[0007] The coating of the present invention adopts water-based phenolic epoxy emulsion and water-based epoxy modified silicone emulsion to improve the compatibility between resins and the high temperature resistance of the coating. It is suitable for the anti-corrosion coating of high-temperature storage tanks of petrochemical intermediate oil and product oil, and solves the problem of discoloration and rust in the existing water-based epoxy coating tank when exposed to high temperature.
[0008] The coating of the present invention uses an aqueous single-walled carbon nanotube solution as a conductive agent, with a small addition amount, and no anti-rust pigment is added, thereby improving the electrostatic conductivity of the coating and making the electrostatic conductivity more stable.
[0009] A first aspect of the present invention provides a water-based high temperature resistant epoxy electrostatic conductive coating.
[0010] A water-based high temperature resistant epoxy electrostatic conductive coating, comprising component A and component B;
[0011] The component A comprises water-based phenolic epoxy emulsion, water-based epoxy-modified silicone emulsion, conductive agent, auxiliary agent and water; the weight ratio of the water-based phenolic epoxy emulsion to the water-based epoxy-modified silicone emulsion is 40-50:(8-15);
[0012] The B component includes a curing agent, an anti-flash rust agent, a co-solvent and water.
[0013] Preferably, the weight ratio of the water-based phenolic epoxy emulsion to the water-based epoxy-modified silicone emulsion is 40-50:(10-15).
[0014] Preferably, the weight ratio of component A to component B is 2-3:1, further 2.2-2.8:1.
[0015] Preferably, the auxiliary agent includes at least one of a dispersant, a defoamer, a pigment, a thickener, a film former, an anti-settling agent or a co-solvent.
[0016] Preferably, the water-based phenolic epoxy emulsion has a solid content greater than or equal to 50%, an epoxy equivalent of 300-400, and trifunctionality.
[0017] Preferably, the particle size of the water-based phenolic epoxy emulsion is less than or equal to 1 micron.
[0018] The water-based phenolic epoxy emulsion can be Baichen Chemical KF-044 or Hansen Epikote 5003.
[0019] Preferably, the solid content of the waterborne epoxy-modified silicone emulsion is 48-52%, and the epoxy equivalent is 1600-2000. The waterborne epoxy-modified silicone emulsion can be SH-9607 silicone emulsion produced by Hubei Longsheng Sihai Company.
[0020] Preferably, the conductive agent is a dispersion of single-walled carbon nanotubes. The dispersion of single-walled carbon nanotubes is MATRIX 302 concentrated solution from TUBALL, which has strong conductivity and has good conductivity even with a low addition amount.
[0021] Preferably, the pigment filler is selected from at least one of iron oxide red, mica powder and barium sulfate.
[0022] Preferably, the defoamer is a mineral oil defoamer and a polysiloxane defoamer, which are used to eliminate bubbles in the membrane. The polysiloxane defoamer is Airex 901W from Digo, which has a high efficiency in defoaming and prevents the generation of bubbles; the mineral oil defoamer is TS-4400 from Ashland, which can quickly break bubbles and eliminate microbubbles in the membrane and has good compatibility.
[0023] Preferably, the curing agent is a mixture of water-based modified polyamide and water-based fatty amine adduct.
[0024] Preferably, in the curing agent, the weight ratio of the water-based modified polyamide to the water-based fatty amine adduct is (1.0-3.5):1, and more preferably (1.5-2.5):1. The water-based modified polyamide has extremely high flexibility and impact resistance, and Huntsman Aradur 340 is selected. The water-based fatty amine adduct has a high molecular weight, good flexibility, and fast drying. The water-based fatty amine adduct is an epoxy addition-polyamine non-ionic water-based curing agent, and Allnex EH2260W / 41WA is selected.
[0025] Preferably, the component A, by weight, comprises 40-50 parts of water-based phenolic epoxy emulsion, 8-15 parts of water-based epoxy-modified silicone emulsion, 0.1-0.4 parts of conductive agent, 20-44.9 parts of auxiliary agent, and 10-15 parts of water; further preferably, the component A, by weight, comprises 40-50 parts of water-based phenolic epoxy emulsion, 10-15 parts of water-based epoxy-modified silicone emulsion, 0.2-0.4 parts of conductive agent, 30.3-44.9 parts of auxiliary agent, and 10-15 parts of water.
[0026] Preferably, the component A comprises, by weight, 40-50 parts of water-based phenolic epoxy emulsion, 10-15 parts of water-based epoxy-modified silicone emulsion, 0.2-0.4 parts of conductive agent, 0.1-0.4 parts of anti-settling agent, 0.3-0.7 parts of dispersant, 15-20 parts of mica powder, 12-18 parts of barium sulfate, 1.5-3 parts of red iron oxide, 0.1-0.8 parts of defoaming agent, 1-2 parts of film-forming agent, 1-3 parts of cosolvent and 10-15 parts of water.
[0027] Preferably, the B component includes, by weight, 22-34 parts of a curing agent, 1-3 parts of an anti-flash rust agent, 2-4 parts of a cosolvent, and 4-8 parts of water.
[0028] The second aspect of the present invention provides a method for preparing a water-based high temperature resistant epoxy electrostatic conductive coating.
[0029] Specifically, a method for preparing a water-based high temperature resistant epoxy electrostatic conductive coating comprises the following steps:
[0030] Preparation of component A: mixing the components to obtain the component A;
[0031] Preparation of component B: mixing the components to obtain the component B;
[0032] The A component and the B component constitute the coating material.
[0033] Preferably, the preparation method comprises the following steps:
[0034] Preparation of component A: Weigh each component, add water, anti-settling agent, defoamer into a dispersion kettle, stir, then add water-based phenolic epoxy emulsion, mica powder, barium sulfate, red iron oxide, stir and sand grind until the fineness reaches 50 microns, stop sand grinding, add water-based epoxy modified silicone emulsion and film-forming aid, stir evenly, and stop stirring after the scraper test fineness and board surface effect are normal, and then obtain component A;
[0035] Preparation of component B: weigh each component, add water-based modified polyamide curing agent, water-based fatty amine adduct, anti-flash rust agent, cosolvent and water into a kettle, stir to obtain component B;
[0036] The A component and the B component constitute the coating material.
[0037] A third aspect of the present invention provides an application of a water-based, high temperature resistant, epoxy electrostatic conductive coating.
[0038] A chemical equipment comprises a coating formed by the above-mentioned water-based high-temperature resistant epoxy static conductive coating.
[0039] Preferably, the chemical equipment includes a storage tank.
[0040] The coating can form a coating on the inner wall of the storage tank, which can increase the service life of the storage tank when storing high-temperature liquids.
[0041] The coating formed by the above-mentioned coating has a good service life at a temperature above 120° C., for example, a long service life in a high temperature environment of 120-200° C.
[0042] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0043] (1) The coating of the present invention uses a specific ratio of water-based phenolic epoxy emulsion and water-based epoxy-modified silicone emulsion to improve the compatibility between resins and the high temperature resistance of the coating. It is suitable for the anti-corrosion coating of high-temperature storage tanks for petrochemical intermediate oils and product oils, and solves the problem of discoloration and rust in existing water-based epoxy coating tanks when exposed to high temperatures.
[0044] (2) The coating of the present invention uses an aqueous single-walled carbon nanotube solution as a conductive agent, with a small amount added and no anti-rust pigment added, thereby improving the electrostatic conductivity of the coating and making the electrostatic conductivity more stable.
[0045] (3) The use of the emulsion in the coating of the present invention in combination with a defoaming agent eliminates bubbles in the film and improves the sealing and rust resistance of the coating; the use of an aqueous dispersion of single-walled carbon nanotubes as a conductive agent has a high cost-effectiveness, simple paint preparation, and good paint film construction performance. DETAILED DESCRIPTION
[0046] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0047] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0048] The sources of raw materials used in the following examples and comparative examples are as follows:
[0049] The water-based phenolic epoxy emulsion is KF-044 from Baichen Chemical.
[0050] The water-based epoxy-modified silicone emulsion is SH-9607 silicone emulsion produced by Hubei Longsheng Sihai Company.
[0051] The conductive agent is a dispersion of single-walled carbon nanotubes, and the dispersion of single-walled carbon nanotubes is a concentrated solution of MATRIX302 produced by TUBALL.
[0052] The defoamers are mineral oil defoamer and polysiloxane defoamer. The polysiloxane defoamer is Airex 901W from Digo Company, and the mineral oil defoamer is TS-4400 from Ashland Company.
[0053] The water-based modified polyamide uses Huntsman Aradur 340. The water-based fatty amine adduct uses Allnex EH2260W / 41WA.
[0054] The anti-settling agent used is Coapur XS-71 from France.
[0055] The dispersant used was German Digo Dispers 760W.
[0056] The co-solvent is Dow Chemical alcohol ester twelve.
[0057] The anti-flash rust agent is Hemmings special chemical NALZIN FA 179.
[0058] Example 1
[0059] A water-based high temperature resistant epoxy electrostatic conductive coating, comprising component A and component B;
[0060] Component A, by weight, consists of 13 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoamer 1# (polysiloxane defoamer), 0.5 parts of dispersant, 40 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, 2 parts of red iron oxide, 10 parts of water-based epoxy-modified silicone emulsion, 0.3 parts of conductive agent, 0.4 parts of defoamer 2# (mineral oil defoamer) and 1 part of cosolvent;
[0061] Component B, by weight, consists of 20 parts of water-based modified polyamide, 10 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent, and 4 parts of water;
[0062] The weight ratio of component A to component B is 2.5:1.
[0063] A method for preparing a water-based high temperature resistant epoxy electrostatic conductive coating comprises the following steps:
[0064] Preparation of component A: by weight, add 13 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoamer 1# (polysiloxane defoamer), and 0.5 parts of dispersant, stir evenly, and stir at high speed (2000 rpm) for 30 minutes, then add 40 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, and 2 parts of red iron oxide, stir evenly, and sand grind until the fineness reaches 50 microns, stop sand grinding, add 10 parts of water-based epoxy modified silicone emulsion, 0.3 parts of conductive agent, 0.4 parts of defoamer 2# (mineral oil defoamer) and 1 part of cosolvent, stir at low speed (800 rpm) for 30 minutes, filter, and package.
[0065] Preparation of component B: add 20 parts of water-based modified polyamide, 10 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent and 4 parts of water into a kettle, stir at 1000r / min for 20min to obtain component B;
[0066] Component A and component B constitute the coating.
[0067] Example 2
[0068] A water-based high temperature resistant epoxy electrostatic conductive coating, comprising component A and component B;
[0069] Component A, by weight, consists of 10 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoamer 1# (polysiloxane defoamer), 45 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, 2 parts of red iron oxide, 10 parts of water-based epoxy-modified silicone emulsion, 0.2 parts of conductive agent, 0.4 parts of defoamer 2# (mineral oil defoamer) and 1 part of cosolvent;
[0070] Component B, by weight, consists of 22 parts of water-based modified polyamide, 13 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent, and 4 parts of water;
[0071] The weight ratio of component A to component B is 2:1.
[0072] A method for preparing a water-based high temperature resistant epoxy electrostatic conductive coating comprises the following steps:
[0073] Preparation of component A: by weight, add 10 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoamer 1# (polysiloxane defoamer), stir evenly, and stir at high speed (2000 rpm) for 30 minutes, then add 45 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, and 2 parts of red iron oxide, stir evenly, and sand grind to a fineness of 50 microns, stop sand grinding, add 10 parts of water-based epoxy-modified silicone emulsion, 0.2 parts of conductive agent, 0.4 parts of defoamer 2# (mineral oil defoamer) and 1 part of cosolvent, stir at low speed (800 rpm) for 30 minutes, filter, and package.
[0074] Preparation of component B: 22 parts of water-based modified polyamide curing agent, 13 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent and 4 parts of water were added into a kettle and stirred at 1000 r / min for 20 minutes to obtain component B;
[0075] Component A and component B constitute the coating.
[0076] Example 3
[0077] A water-based high temperature resistant epoxy electrostatic conductive coating, comprising component A and component B;
[0078] Component A, by weight, consists of 13 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoamer 1# (polysiloxane defoamer), 45 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, 2 parts of red iron oxide, 8 parts of water-based epoxy-modified silicone emulsion, 0.4 parts of conductive agent, 0.5 parts of defoamer 2# (mineral oil defoamer) and 1 part of cosolvent;
[0079] Component B, by weight, consists of 22 parts of water-based modified polyamide, 12 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent, and 4 parts of water;
[0080] The weight ratio of component A to component B is 2.8:1.
[0081] A method for preparing a water-based high temperature resistant epoxy electrostatic conductive coating comprises the following steps:
[0082] Preparation of component A: by weight, add 13 parts of water, 0.4 parts of anti-settling agent, 0.1 parts of defoaming agent 1# (polysiloxane defoaming agent), stir evenly, and stir at high speed (2000 rpm) for 30 minutes, then add 45 parts of water-based phenolic epoxy emulsion, 18 parts of mica powder, 15 parts of barium sulfate, and 2 parts of red iron oxide, stir evenly, and sand grind to a fineness of 50 microns, stop sand grinding, add 8 parts of water-based epoxy modified silicone emulsion, 0.4 parts of conductive agent, 0.5 parts of defoaming agent 2# (mineral oil defoaming agent) and 1 part of cosolvent, stir at low speed (1000 rpm) for 30 minutes, filter, and package.
[0083] Preparation of component B: Add 22 parts of water-based modified polyamide curing agent, 12 parts of water-based fatty amine adduct, 1 part of anti-flash rust agent, 2 parts of cosolvent and 4 parts of water into a kettle, stir at 1000r / min for 20min to obtain component B;
[0084] Component A and component B constitute the coating.
[0085] Comparative Example 1
[0086] Compared with Example 1, the difference of Comparative Example 1 is that the amount of water-based phenolic epoxy emulsion is adjusted to 30 parts, the amount of water-based modified polyamide is adjusted to 15 parts, and the other components and processes are the same as those of Example 1.
[0087] Comparative Example 2
[0088] Compared with Example 1, the difference of Comparative Example 2 is that the amount of water-based phenolic epoxy emulsion is adjusted to 50 parts, the amount of water-based modified polyamide is adjusted to 24 parts, and the other components and processes are the same as those of Example 1.
[0089] Comparative Example 3
[0090] Compared with Example 1, the difference in Comparative Example 3 is that the amount of the conductive agent is adjusted to 0 parts, the amount of barium sulfate is adjusted to 0 parts, the amount of mica powder is adjusted to 15 parts, and to ensure that the epoxy equivalent and the active hydrogen equivalent remain consistent, the amount of the water-based modified polyamide curing agent is adjusted to 18 parts, and the amount of the water-based fatty amine adduct is adjusted to 7 parts. The remaining components and processes are the same as those in Example 1.
[0091] Comparative Example 4
[0092] Compared with Example 1, the difference of Comparative Example 4 is that the amount of water-based phenolic epoxy emulsion is adjusted to 30 parts, the amount of water-based epoxy-modified silicone emulsion is adjusted to 20 parts, and the amount of water-based modified polyamide is adjusted to 16 parts. The other components and processes are the same as those in Example 1.
[0093] Product effect testing
[0094] The performance of the coatings prepared in the above embodiments and comparative examples (mixing component A and component B to obtain a coating, applying, and drying under natural conditions for 24 hours to form a film layer) was tested according to the test standards shown in Table 1. The test results are shown in Tables 2 and 3.
[0095] Table 1
[0096]
[0097]
[0098] Table 2
[0099]
[0100]
[0101] Table 3
[0102]
[0103]
[0104] It can be seen from Table 2-3 that the coating formed by the coating prepared in the embodiment of the present invention has good high temperature resistance and corrosion resistance.
Claims
1. A coating, It is characterized in that It includes component A and component B; The component A comprises water-based phenolic epoxy emulsion, water-based epoxy-modified silicone emulsion, conductive agent, auxiliary agent and water; the weight ratio of the water-based phenolic epoxy emulsion to the water-based epoxy-modified silicone emulsion is 40-50:(8-15); The B component includes a curing agent, an anti-flash rust agent, a co-solvent and water.
2. The coating according to claim 1, It is characterized in that The weight ratio of component A to component B is 2-3:
1.
3. The coating according to claim 1, It is characterized in that The auxiliary agent includes at least one of a dispersant, a defoamer, a pigment filler, a defoamer, a thickener, a film former, an anti-settling agent or a co-solvent.
4. The coating according to claim 1, It is characterized in that The water-based phenolic epoxy emulsion has a solid content greater than or equal to 50%, an epoxy equivalent of 300-400, and trifunctionality; and / or the water-based epoxy-modified silicone emulsion has a solid content of 48-52%, and an epoxy equivalent of 1600-2000.
5. The coating according to claim 1, It is characterized in that The conductive agent is a dispersion of single-walled carbon nanotubes.
6. The coating according to claim 1, It is characterized in that The curing agent is a mixture of water-based modified polyamide and water-based fatty amine adduct.
7. The coating according to claim 1, It is characterized in that The component A comprises, by weight, 40-50 parts of water-based phenolic epoxy emulsion, 8-15 parts of water-based epoxy-modified silicone emulsion, 0.1-0.4 parts of conductive agent, 20-44.9 parts of auxiliary agent and 10-15 parts of water.
8. The coating according to claim 1, It is characterized in that The auxiliary agents include dispersants, defoamers, pigments and fillers, film formers, anti-settling agents and cosolvents, and the pigments and fillers include mica powder, barium sulfate and red iron oxide; the component A, by weight, includes 40-50 parts of water-based phenolic epoxy emulsion, 10-15 parts of water-based epoxy-modified silicone emulsion, 0.2-0.4 parts of conductive agent, 0.1-0.4 parts of anti-settling agent, 0.3-0.7 parts of dispersant, 15-20 parts of mica powder, 12-18 parts of barium sulfate, 1.5-3 parts of red iron oxide, 0.1-0.8 parts of defoamers, 1-2 parts of film formers, 1-3 parts of cosolvents, and 10-15 parts of water; And / or, the B component, by weight, includes 22-34 parts of a curing agent, 1-3 parts of an anti-flash rust agent, 2-4 parts of a cosolvent, and 4-8 parts of water.
9. A method for preparing a coating according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Preparation of component A: mixing the components to obtain the component A; Preparation of component B: mixing the components to obtain the component B; The A component and the B component constitute the coating material.
10. A chemical equipment, It is characterized in that A coating formed by the coating material according to any one of claims 1 to 8.
Citation Information
Patent Citations
Water-based phenolic epoxy static conductive coating for long-acting protection and preparation method of water-based phenolic epoxy static conductive coating
CN115286976A
Water-based static conductive coating for storage tank and preparation method of water-based static conductive coating
CN115820075A
Temperature-resistance thermal-insulation heavy-duty anticorrosion coating
CN102134444A
Water-based epoxy anticorrosive paint for containers, and preparation method and application thereof
CN112646455A
Water-based phenolic epoxy coating material and preparation method thereof
CN113980550A