Ethanol-driven rapid bonding method for dissimilar materials
The ethanol-driven method using a polylactic acid composite adhesive layer sheet addresses slow bonding speeds by ensuring uniform penetration and high strength adhesion for dissimilar materials.
Patent Information
- Application Number
- CN202411369196.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-29
AI Technical Summary
Existing adhesives for bonding dissimilar materials have high viscosity, poor fluidity, and difficulty penetrating gaps, leading to slow bonding speeds and uneven distribution, affecting the bonding process.
An ethanol-driven method using a polylactic acid composite adhesive layer sheet prepared with specific ratios of polylactic acid polyol, isocyanate, anhydrous organic solvent, and catalyst, soaked in ethanol to facilitate rapid bonding by applying vertical pressure until ethanol evaporates.
Achieves uniform and rapid adhesive application with bonding strengths exceeding 2MPa under minimal pressure, suitable for various dissimilar materials like wood, bamboo, steel, glass, and ceramics.
Smart Images

Figure CN119081557A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dissimilar material bonding methods, and in particular relates to an ethanol-driven dissimilar material rapid bonding method. Background Art
[0002] Dissimilar material bonding refers to the process of connecting two or more different materials into a whole through adhesives or other connection technologies. These materials differ in chemical composition, metallographic structure, physical properties or mechanical properties. Dissimilar material bonding technology is widely used in aerospace, automobile manufacturing, electronic appliances, medical equipment, construction engineering and other fields, and is of great significance for improving the comprehensive performance of products, reducing weight and reducing costs.
[0003] Common methods for bonding dissimilar materials include adhesive bonding, welding, mechanical connection, etc. Among them, adhesive bonding is the most common dissimilar bonding method. By selecting a suitable adhesive, a firm connection between materials can be achieved without destroying the performance of the parent material.
[0004] However, existing adhesives used for bonding dissimilar materials often have high viscosity, poor fluidity, and are difficult to penetrate into the gaps of dissimilar materials, which slows down the bonding speed. In addition, the method and uniformity of glue application will also affect the distribution and penetration effect of the adhesive, thereby affecting the bonding speed. Summary of the invention
[0005] In order to solve the problem that the existing adhesive has a slow bonding speed when used for bonding dissimilar materials, the present invention provides an ethanol-driven method for fast bonding dissimilar materials.
[0006] The technical solution of the present invention:
[0007] An ethanol-driven method for rapid bonding of dissimilar materials comprises the following steps:
[0008] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0009] Step 2, soaking the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution to drive bonding;
[0010] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the dissimilar materials to be bonded, and apply a certain vertical pressure to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0011] Furthermore, the raw materials for preparing the polylactic acid composite adhesive layer sheet in step 1 include polylactic acid polyol, isocyanate, anhydrous organic solvent, catalyst and chain extender; wherein the mass volume ratio of polylactic acid polyol, isocyanate, anhydrous organic solvent and chain extender is 8-10g:1-3g:80-120ml:0.1-1.5g, and the amount of the catalyst is 0.3% of the total mass of polylactic acid polyol and isocyanate.
[0012] Furthermore, the polylactic acid polyol is one or a combination of polylactic acid polyols having a molecular weight of 500 to 2000.
[0013] Furthermore, the isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate; and the anhydrous organic solvent is one of butanone, dioxane, N,N-dimethylformamide or dimethylacetamide.
[0014] Furthermore, the catalyst is a tin-based catalyst, specifically stannous octoate or stannous chloride; the chain extender is one or a combination of sebacic acid dihydrazide, succinic acid dihydrazide, and 2,5-bis(benzyloxy)terephthaloylhydrazide.
[0015] Furthermore, the preparation method of the polylactic acid composite adhesive layer sheet is as follows: polylactic acid polyol, isocyanate and catalyst are placed in an inert atmosphere, and reacted at a temperature of 70 to 90° C. for 3 to 5 hours to obtain a prepolymer; an anhydrous organic solvent and a chain extender are added to the obtained prepolymer, and the reaction temperature is reduced to room temperature and then continued to react for 24 to 48 hours in an inert atmosphere to obtain a composite system; the obtained composite system is poured into a mold, and after standing at room temperature, the anhydrous organic solvent in the composite system is volatilized and removed to obtain a polylactic acid composite adhesive layer sheet.
[0016] Furthermore, the thickness of the obtained polylactic acid composite adhesive layer sheet is 0.02-2 mm.
[0017] Furthermore, in step 2, the volume concentration of the ethanol solution is 50-100%, and the infiltration time is 10-60 seconds.
[0018] Furthermore, the heterogeneous materials described in step three include wood, bamboo, iron, aluminum, copper, stainless steel, glass, ceramics, plastic and rubber.
[0019] Furthermore, the pressure is not less than 5000Pa.
[0020] Beneficial effects of the present invention:
[0021] The bonding method provided by the present invention uses the polylactic acid composite adhesive layer of the sheet as an adhesive, uses ethanol to drive the rapid bonding performance of the polylactic acid composite adhesive layer, and spreads it between the heterogeneous materials to be bonded, which is not only easy to achieve uniform and rapid adhesive application, but also can achieve a bonding strength of more than 2MPa under very small pressure. The ethanol-driven heterogeneous material rapid bonding method of the present invention can be applied to heterogeneous bonding of wood, bamboo, steel, glass, ceramics, etc., and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a comparison chart of the bonding strength of different dissimilar materials bonded by the quick bonding method in Examples 1 to 5;
[0023] Figure 2 This is a physical demonstration diagram of the bonding strength of bamboo pieces and iron pieces bonded by the quick bonding method provided in Example 1. The weight of the dumbbell in the figure is 10 kg. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0025] Example 1
[0026] This embodiment provides an ethanol-driven method for rapid bonding of dissimilar materials, comprising the following steps:
[0027] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0028] First, 8.82g of polylactic acid polyol PLA-OH was weighed into a four-necked flask connected to a vacuum pump, and the water was removed by stirring. Then, 1.03g of IPDI and 0.3% of the total weight of polylactic acid polyol and isocyanate stannous octoate were added, nitrogen was introduced, and the mixture was reacted at 80°C for 3.5h to obtain a prepolymer; 100ml of butanone was added to the obtained prepolymer to reduce the viscosity of the reaction system, and after the system was cooled to room temperature of 25°C, 0.11g of IPDH was added to carry out a chain extension reaction, and nitrogen was introduced throughout the reaction for 12h to obtain a composite system; the obtained composite system was poured into a mold, allowed to stand at room temperature overnight, and then placed in a 50°C oven for 24h to volatilize and remove the butanone in the composite system, thereby obtaining a polylactic acid composite adhesive layer sheet with a thickness of 0.2mm.
[0029] Step 2: Immerse the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution with a volume concentration of 100% for 30 seconds to drive bonding;
[0030] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the two dissimilar materials that need to be bonded, namely the bamboo piece and the iron sheet, and apply a vertical pressure of 5000 Pa to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0031] Example 2
[0032] This embodiment provides an ethanol-driven method for rapid bonding of dissimilar materials, comprising the following steps:
[0033] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0034] First, 8.82g of polylactic acid polyol PLA-OH was weighed into a four-necked flask connected to a vacuum pump, and the water was removed by stirring. Then, 1.03g of IPDI and 0.3% of the total weight of polylactic acid polyol and isocyanate stannous octoate were added, nitrogen was introduced, and the mixture was reacted at 80°C for 3.5h to obtain a prepolymer; 100ml of butanone was added to the obtained prepolymer to reduce the viscosity of the reaction system, and after the system was cooled to room temperature of 25°C, 0.11g of IPDH was added to carry out a chain extension reaction, and nitrogen was introduced throughout the reaction for 12h to obtain a composite system; the obtained composite system was poured into a mold, allowed to stand at room temperature overnight, and then placed in a 50°C oven for 24h to volatilize and remove the butanone in the composite system, thereby obtaining a polylactic acid composite adhesive layer sheet with a thickness of 0.2mm.
[0035] Step 2: Immerse the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution with a volume concentration of 100% for 30 seconds to drive bonding;
[0036] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the two dissimilar materials that need to be bonded, namely the bamboo piece and the ceramic, and apply a vertical pressure of 5000 Pa to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0037] Example 3
[0038] This embodiment provides an ethanol-driven method for rapid bonding of dissimilar materials, comprising the following steps:
[0039] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0040] First, 8.82g of polylactic acid polyol PLA-OH was weighed into a four-necked flask connected to a vacuum pump, and the water was removed by stirring. Then, 1.03g of IPDI and 0.3% of the total weight of polylactic acid polyol and isocyanate stannous octoate were added, nitrogen was introduced, and the mixture was reacted at 80°C for 3.5h to obtain a prepolymer; 100ml of butanone was added to the obtained prepolymer to reduce the viscosity of the reaction system, and after the system was cooled to room temperature of 25°C, 0.11g of IPDH was added to carry out a chain extension reaction, and nitrogen was introduced throughout the reaction for 12h to obtain a composite system; the obtained composite system was poured into a mold, allowed to stand at room temperature overnight, and then placed in a 50°C oven for 24h to volatilize and remove the butanone in the composite system, thereby obtaining a polylactic acid composite adhesive layer sheet with a thickness of 0.2mm.
[0041] Step 2: Immerse the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution with a volume concentration of 100% for 30 seconds to drive bonding;
[0042] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the two dissimilar materials that need to be bonded, namely the bamboo piece and the glass, and apply a vertical pressure of 5000 Pa to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0043] Example 4
[0044] This embodiment provides an ethanol-driven method for rapid bonding of dissimilar materials, comprising the following steps:
[0045] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0046] First, 8.82g of polylactic acid polyol PLA-OH was weighed into a four-necked flask connected to a vacuum pump, and the water was removed by stirring. Then, 1.03g of IPDI and 0.3% of the total weight of polylactic acid polyol and isocyanate stannous octoate were added, nitrogen was introduced, and the mixture was reacted at 80°C for 3.5h to obtain a prepolymer; 100ml of butanone was added to the obtained prepolymer to reduce the viscosity of the reaction system, and after the system was cooled to room temperature of 25°C, 0.11g of IPDH was added to carry out a chain extension reaction, and nitrogen was introduced throughout the reaction for 12h to obtain a composite system; the obtained composite system was poured into a mold, allowed to stand at room temperature overnight, and then placed in a 50°C oven for 24h to volatilize and remove the butanone in the composite system, thereby obtaining a polylactic acid composite adhesive layer sheet with a thickness of 0.2mm.
[0047] Step 2: Immerse the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution with a volume concentration of 100% for 30 seconds to drive bonding;
[0048] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the two dissimilar materials that need to be bonded, namely the bamboo piece and the stainless steel, and apply a vertical pressure of 5000 Pa to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0049] Example 5
[0050] This embodiment provides an ethanol-driven method for rapid bonding of dissimilar materials, comprising the following steps:
[0051] Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material;
[0052] First, 8.82g of polylactic acid polyol PLA-OH was weighed into a four-necked flask connected to a vacuum pump, and the water was removed by stirring. Then, 1.03g of IPDI and 0.3% of the total weight of polylactic acid polyol and isocyanate stannous octoate were added, nitrogen was introduced, and the mixture was reacted at 80°C for 3.5h to obtain a prepolymer; 100ml of butanone was added to the obtained prepolymer to reduce the viscosity of the reaction system, and after the system was cooled to room temperature of 25°C, 0.11g of IPDH was added to carry out a chain extension reaction, and nitrogen was introduced throughout the reaction for 12h to obtain a composite system; the obtained composite system was poured into a mold, allowed to stand at room temperature overnight, and then placed in a 50°C oven for 24h to volatilize and remove the butanone in the composite system, thereby obtaining a polylactic acid composite adhesive layer sheet with a thickness of 0.2mm.
[0053] Step 2: Immerse the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution with a volume concentration of 100% for 30 seconds to drive bonding;
[0054] Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the two dissimilar materials that need to be bonded, namely the bamboo and wood chips, and apply a vertical pressure of 5000 Pa to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
[0055] Figure 1 The bonding strength comparison diagram of different dissimilar materials bonded by the rapid bonding method in Examples 1-5 shows that the bonding strength of the two dissimilar materials of bamboo and iron in Example 1 is 6.4±1.2MPa; the bonding strength of the two dissimilar materials of bamboo and ceramic in Example 2 is 6.3±1.6MPa; the bonding strength of the two dissimilar materials of bamboo and glass in Example 3 is 2.6±0.7MPa; the bonding strength of the two dissimilar materials of bamboo and stainless steel in Example 4 is 5.3±1.2MPa; the bonding strength of the two dissimilar materials of bamboo and wood in Example 5 is 11.8±1.1MPa. It can be proved that the ethanol-driven dissimilar material rapid bonding method provided by the present invention has a good dissimilar material bonding effect, and the bonding strength can reach up to 11.8MPa.
Claims
1. An ethanol-driven method for rapid bonding of dissimilar materials, characterized in that: The steps include: Step 1, preparing a polylactic acid composite adhesive layer sheet using polylactic acid polyol as a raw material; Step 2, soaking the polylactic acid composite adhesive layer sheet obtained in step 1 in an ethanol solution to drive bonding; Step 3: Lay the polylactic acid composite adhesive layer sheet that has been soaked in step 2 between the dissimilar materials to be bonded, and apply a certain vertical pressure to the bonding surface until the ethanol evaporates completely, thus completing the bonding.
2. According to claim 1, an ethanol-driven method for rapid bonding of dissimilar materials is characterized in that: The raw materials for preparing the polylactic acid composite adhesive layer sheet in step 1 include polylactic acid polyol, isocyanate, anhydrous organic solvent, catalyst and chain extender; wherein the mass volume ratio of polylactic acid polyol, isocyanate, anhydrous organic solvent and chain extender is 8-10g:1-3g:80-120ml:0.1-1.5g, and the amount of the catalyst is 0.3% of the total mass of polylactic acid polyol and isocyanate.
3. The ethanol-driven rapid bonding method of dissimilar materials according to claim 2, characterized in that: The polylactic acid polyol is one or a combination of polylactic acid polyols having a molecular weight of 500 to 2000.
4. The ethanol-driven rapid bonding method of dissimilar materials according to claim 3, characterized in that: The isocyanate is one or a combination of polymethylene polyphenyl isocyanate, toluene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate or lysine diisocyanate; and the anhydrous organic solvent is one of butanone, dioxane, N,N-dimethylformamide or dimethylacetamide.
5. The ethanol-driven rapid bonding method of dissimilar materials according to claim 4, characterized in that: The catalyst is a tin-based catalyst, specifically stannous octoate or stannous chloride; the chain extender is one or a combination of sebacic acid hydrazide, succinic acid dihydrazide, and 2,5-bis(benzyloxy)terephthaloylhydrazide.
6. An ethanol-driven method for rapid bonding of dissimilar materials according to any one of claims 1 to 5, characterized in that: The preparation method of the polylactic acid composite adhesive layer sheet is as follows: polylactic acid polyol, isocyanate and catalyst are placed in an inert atmosphere, reacted at a temperature of 70 to 90° C. for 3 to 5 hours to obtain a prepolymer; an anhydrous organic solvent and a chain extender are added to the obtained prepolymer, the reaction temperature is reduced to room temperature, and the reaction is continued for 24 to 48 hours in an inert atmosphere to obtain a composite system; the obtained composite system is poured into a mold, and after standing at room temperature, the anhydrous organic solvent in the composite system is volatilized and removed to obtain the polylactic acid composite adhesive layer sheet.
7. The ethanol-driven rapid bonding method of dissimilar materials according to claim 6, characterized in that: The thickness of the obtained polylactic acid composite adhesive layer sheet is 0.02-2 mm.
8. The ethanol-driven rapid bonding method of dissimilar materials according to claim 7, characterized in that: In step 2, the volume concentration of the ethanol solution is 50-100%, and the infiltration time is 10-60s.
9. The ethanol-driven rapid bonding method of dissimilar materials according to claim 8, characterized in that: The heterogeneous materials described in step 3 include wood, bamboo, iron, aluminum, copper, stainless steel, glass, ceramics, plastic and rubber.
10. The ethanol-driven rapid bonding method of dissimilar materials according to claim 9, characterized in that: The pressure is not less than 5000Pa.
Citation Information
Patent Citations
Self-repairing waterborne polyurethane film and preparation method thereof
CN116355249A
Alcohol-soluble polyurethane-coating agent, adhesive, and leather like sheet prepared by using them
JP2011042756A
Cited By
Ethanol-driven rapid bonding method for dissimilar materials
WO2026066520A1