Slag system for gas protection electroslag remelting as well as preparation method and use method of slag system
By using pre-slag composition at different melting points in electroslag remelting and controlling its joining order, the problem of consumable electrode melting caused by solid slag start is solved, and the bottom surface quality and production efficiency of high-temperature alloy electroslag ingots are improved.
Patent Information
- Application Number
- CN202411195603.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
During the gas-protected electroslag remelting process, solid slag starts to melt the consumable electrode, causing poor surface quality at the bottom of the high-temperature alloy electroslag ingot.
The first component premelting slag and the second component premelting slag are composed of two different melting points. The first component premelting slag and the second component premelting slag are respectively at melting points of 960-1100°C and 1200-1300°C, respectively, and the addition order is controlled. The slag phase is added to the crystallizer in batches, and the melting process is optimized to prevent melting of the consumable electrode.
Effectively prevent the melting of self-consumable electrodes, ensure good surface quality of the bottom surface of the electroslag ingot, reduce production costs, and improve the overall quality of the high-temperature alloy electroslag ingot.
Smart Images

Figure CN119082471A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electroslag metallurgy, and more specifically to a slag system for gas-protected electroslag remelting and a preparation and use method thereof. Background Art
[0002] In the process of electroslag remelting, there are two main arc starting methods: liquid slag start and solid slag start. Liquid slag start is to melt the prepared slag in another set of slag melting furnace, then pour it into the crystallizer, turn on the power and start remelting. Solid slag start refers to slag melting in the crystallizer. When the end of the metal electrode contacts the conductive slag, the slag is evenly added to the crystallizer. After the slag is melted, the remelting stage can be entered. At present, in order to improve the cleanliness of high-temperature alloy electroslag ingots and reduce the burn-in of easily oxidized elements, a gas-protected remelting method is often used, that is, a protective cover is added above the crystallizer, and an inert gas such as Ar is introduced into the protective cover during the remelting process to shield the air from pollution. Because a protective cover is installed above the crystallizer, the liquid slag melted in the slag melting furnace cannot or is difficult to be poured into the crystallizer, resulting in the inability to use the liquid slag start method for arc starting. Therefore, for gas-protected electroslag remelting, solid slag start is often used.
[0003] However, solid slag startup has a significant disadvantage, that is, the solid slag melting process is often accompanied by the melting of the consumable electrode. As a result, the slag skin on the lower surface of the electroslag ingot is very thick and the surface quality is very poor. Therefore, the bottom of the electroslag ingot has to be cut off. This is a huge waste for expensive high-temperature alloys, resulting in increased production costs. Therefore, it is particularly necessary to improve the bottom surface quality of high-temperature alloy electroslag ingots under solid slag startup conditions. The common operation is to add mixed slag to the crystallizer in batches, or to add the slag to the crystallizer in sequence according to the components of the slag, but the above operations cannot control the temperature during the slag melting process well, and thus cannot prevent the consumable electrode from melting during the arc starting stage.
[0004] After searching, the application of Chinese Patent No. 2021100702292 discloses a method for preparing electroslag remelted low-oxygen titanium-containing steel by pre-melted slag and deoxidation for electroslag remelting titanium-containing steel. It discloses that the pre-melted slag for electroslag remelting titanium-containing steel is composed of A pre-melted slag and B pre-melted slag. The main difference between the components of A pre-melted slag and B pre-melted slag is whether it contains titanium dioxide. It also discloses a calculation formula for determining the mass percentage of A pre-melted slag and B pre-melted slag in the slag system according to the content of titanium and aluminum elements in the consumable electrode, which solves the technical problems of how to determine the amount of titanium dioxide added when smelting titanium-containing steel using electroslag remelting technology, the volatility of titanium dioxide during the addition process, and the unevenness of titanium dioxide in the slag system. At the same time, steels with different titanium contents can be smelted by the ratio of A pre-melted slag and B pre-melted slag, thereby improving the quality stability of the slag system. However, this application still cannot solve the problem of how to prevent the melting of the consumable electrode during the slag smelting process. Summary of the invention
[0005] In view of the technical problem that the consumable electrode melts during the slag melting process, which easily leads to poor surface quality at the bottom of the high-temperature alloy, this solution provides a slag system for gas-shielded electroslag remelting and a preparation and use method thereof. The slag system includes a first component pre-melted slag and a second component pre-melted slag with different melting points. By controlling the addition order of the first component pre-melted slag and the second component pre-melted slag, the slag system melting process at the arc starting stage of the slag system can be optimized, thereby ensuring good surface quality at the bottom of the electroslag ingot.
[0006] To achieve the above-mentioned purpose, the first aspect of the present invention provides a slag system for gas shielded electroslag remelting, the slag system comprising a first component pre-melted slag and a second component pre-melted slag, wherein, in terms of mass percentage of the entire slag system: the first component pre-melted slag comprises the following components: cryolite 18%-26%, Al2O3 5%-10%, CaF2 10%-15%, MgF2 10%-15%, NaF 2-4%, AlF3 1-2%; the melting point of the first component pre-melted slag is 960-1100°C; the second component pre-melted slag comprises the following components: Al2O3 5%-15%, CaF2 5%-20%, MgF2 5%-20%, TiO2 2%-10%, CaO 5% to 10%; the melting point of the second component pre-melted slag is 1200 to 1300°C, and the first component pre-melted slag and the second component pre-melted slag are used to be added to the crystallizer in batches during the arcing and slagging stage.
[0007] The present invention optimizes the slag system composition of electroslag remelting, designs it to contain two pre-melted slag compositions with different melting points, and adds them to the crystallizer in batches during the arcing and slagging stage, thereby effectively preventing the consumable electrode from melting, which is beneficial to ensuring the bottom quality of the electroslag ingot. Specifically, the mass percentage of the first component pre-melted slag in the entire slag system reaches 46% to 72%, and its melting point is only 960 to 1100°C. The required slag-melting temperature is relatively low, and the slag-melting temperature is lower than the melting point of the consumable electrode. Therefore, the first component pre-melted slag is first added to the crystallizer during the arcing and slagging stage, and the second component pre-melted slag is added after the first component pre-melted slag is completely melted, thereby ensuring that the consumable electrode does not melt during the arcing and slagging stage, and ensuring the surface quality of the bottom of the high-temperature alloy electroslag ingot.
[0008] Furthermore, the overall slag system composed of the first component pre-melted slag and the second component pre-melted slag includes the following components in mass percentage: cryolite 18%-26%, Al2O3 15-20%, TiO2 2%-10%, CaF2 20%-30%, MgF220%-30%, CaO 5%-10%, NaF 2-4%, and AlF3 1-2%.
[0009] By optimizing the ratio of the first component pre-melted slag and the second component pre-melted slag, the composition of the overall slag system can be controlled, which can not only effectively prevent the melting of the consumable electrode during the arcing and slagging stage, but also effectively ensure the quality of the electroslag remelting product, especially to make the slag system meet the electroslag remelting requirements of high-temperature nickel-based alloys. Specifically, the melting point of the slag system is 1150-1250°C, the viscosity is 0.12-0.24Pa.s, and the conductivity is 2.5-3.5S.cm -1 The stability of the slag system is 1.69-1.75. The melting point and viscosity of the overall slag system are low, and the stability is good.
[0010] The calculation formula for slag system stability is: M=1.61*n(Al2O3)+2.16*n(CaO)+1.14*n(TiO2), where n(Al2O3), n(CaO), and n(TiO2) are the molar ratios of Al2O3, CaO, and TiO2 in the slag system, respectively. In the above formula, M represents stability.
[0011] Specifically, based on the comprehensive consideration of the overall slag system performance requirements and the prevention of consumable electrode melting, since cryolite, NaF, and AlF3 can effectively reduce the melting point of the pre-melted slag, they are added to the first component pre-melted slag to reduce the melting point of the first component pre-melted slag; and CaO has a high melting point, low resistance, and will increase the viscosity of the slag system, so it is added to the second component pre-melted slag. In addition, although CaF2 and MgF2 can reduce the melting point, they will reduce the resistance of the slag system, and although Al2O3 has a higher melting point, it can increase the resistance of the slag and stabilize the arc starting current. Therefore, part of CaF2, MgF2 and Al2O3 are added to the first component pre-melted slag and the second component pre-melted slag respectively, so as to meet the requirements of the pre-melted slag for melting point and resistance as much as possible. Furthermore, in order to prevent oxygen from passing through the slag pool through TiO2 and then entering the high-temperature alloy, TiO2 is placed in the second component pre-melted slag.
[0012] Furthermore, the particle sizes of the first component pre-melted slag and the second component pre-melted slag are 5-15mm and 2-5mm, respectively. There is dust removal treatment during the arc starting stage. If the particle size of the first component pre-melted slag is too small, part of the slag will be sucked away by the dust removal, resulting in a deviation in the slag system composition and affecting the overall performance of the slag; at the same time, since the temperature required for slag slag of the first component pre-melted slag is relatively low, a slightly larger particle size of the first pre-melted slag will not affect the slag slag efficiency, so the particle size of the first component pre-melted slag is more suitable between 5 and 15mm. In addition, after the first component pre-melted slag is completely melted, the second component pre-melted slag with a relatively high melting point is added. The smaller particle size of the second component pre-melted slag is more conducive to its melting, and since the amount of dust is less at this time, the dust removal and ventilation strength is relatively small, even if the particle size is slightly smaller, the slag will not be taken away. In actual use, the particle size of the second pre-melted slag is more suitable between 2 and 5mm.
[0013] The second aspect of the present invention provides a method for preparing a slag system for gas-shielded electroslag remelting, comprising: heating and melting a mixture of components of a first-component pre-melted slag, and then cooling and crushing it to obtain a first-component pre-melted slag; heating and melting a mixture of components of a second-component pre-melted slag, and then cooling and crushing it to obtain a second-component pre-melted slag.
[0014] The present invention pre-melts the first component slag and the second component slag. For the first component slag before pre-melting, the melting point of each component is relatively high, for example, the melting point of CaF2 is 1402°C, and the melting point of Al2O3 is as high as 2054°C. If only physical mixing is performed inside each component, no new substance is actually formed. When the physically mixed material is added to the crystallizer, the slag melting temperature must be increased to gradually melt the slag. The higher slag pool temperature will cause the melting of the consumable electrode, that is, the electrode melting cannot be avoided while slagging, which ultimately leads to a thick slag skin on the surface of the prepared electroslag ingot and poor quality. After the components inside each component are mixed and pre-melted, a single-phase slag composed of multiple components is actually formed, and its melting point is reduced. For example, the melting point of the first pre-melted slag component is only 960-1100°C, and the melting speed in the crystallizer is faster.
[0015] Furthermore, the heating and melting temperature of the first component pre-melted slag is 1200-1300°C, and the heating and melting temperature of the second component pre-melted slag is 1300-1500°C.
[0016] A third aspect of the present invention provides a method for using a slag system for gas-shielded electroslag remelting, comprising:
[0017] (1) Arcing and powering on; the control voltage is 22-28V, the current is 3000-4000A, and the first component pre-melted slag is first added into the crystallizer for melting, and the slag melting temperature does not exceed 1250°C;
[0018] (2) After the first component pre-melted slag is melted, the voltage is controlled to be 28-32V and the current is 5000-6500A, and then the second component pre-melted slag is added to the crystallizer for melting;
[0019] (3) After the second component pre-melted slag is melted, the voltage is controlled to 30-32V and the current is 6000-7000A to carry out the normal remelting stage.
[0020] In the above-mentioned method of use: in step 1), because the melting point and resistance of the first component pre-melted slag are both relatively low, by controlling the appropriate slag-melting current and voltage, the slag material can be fully melted without making the slag-melting temperature too high, thereby preventing the consumable electrode from melting; in step 2), the melting point of the second component pre-melted slag is relatively high, and in order to completely melt the slag material, it is necessary to appropriately increase the power parameter at this time; since the second component pre-melted slag is added on the basis of the complete melting of the first component pre-melted slag and the second component pre-melted slag has a smaller particle size, it is helpful for it to melt quickly in the crystallizer, and thus the consumable electrode is basically not melted or the amount of melting is very small; in step 3), after the slag is completely melted, since the consumable electrode has a relatively high melting point, the supplied power is gradually increased at this time, the slag pool temperature is increased, the consumable electrode begins to melt, and the normal remelting stage is carried out.
[0021] Furthermore, the melting time of the first component pre-melted slag is 30 to 60 minutes.
[0022] Furthermore, the melting time of the second component pre-melted slag is 10 to 20 minutes.
[0023] Furthermore, the crystallizer includes a lower crystallizer and an upper crystallizer, both of which are arranged along the axial direction of the consumable electrode. The height of the lower crystallizer is 200-300 mm, which is slightly higher than the height of the slag pool. In the arcing and slagging stage, the temperature difference between the inlet and outlet cooling water of the upper crystallizer is 10-20°C and the outlet water temperature does not exceed 40°C, and the temperature difference between the inlet and outlet cooling water of the lower crystallizer is 30-40°C, and the outlet water temperature does not exceed 70°C. The slagging process is carried out in the lower crystallizer, and the temperature difference between the inlet and outlet of the lower crystallizer is large, which can prevent the slag pool temperature from dropping rapidly, is beneficial to the uniformity of the slag temperature in the crystallizer, and helps to melt the slag quickly. At this stage, the inner wall of the upper crystallizer is a free space. At this time, reducing the temperature difference between the inlet and outlet water of the upper crystallizer can reduce the temperature of the copper plate on the inner wall of the crystallizer, thereby reducing the temperature of the gas contacting the inner wall copper plate and changing the density, promoting the enhancement of gas convection movement inside the crystallizer, and facilitating the protective gas introduced into the crystallizer to quickly bring out the air, thereby reducing the impact of air on the quality of the electroslag ingot; 1 hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer is adjusted to 10-20°C, and the outlet water temperature does not exceed 40°C. By reducing the inlet and outlet water temperature difference of the lower crystallizer, the cooling rate of the lower crystallizer is increased, the depth of the metal molten pool is reduced, the cooling of the electroslag ingot is accelerated, and thus it helps to improve the quality of the electroslag ingot.
[0024] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0025] (1) The present invention provides a slag system for gas-shielded electroslag remelting. The composition of the slag system is optimized to include two pre-melted slag components with different melting points: a first-component pre-melted slag and a second-component pre-melted slag. When arcing and slagging, the first-component pre-melted slag is added first, and then the second-component pre-melted slag is added. This can effectively optimize the slag system melting process in the arcing stage, prevent the consumable electrode from melting in the arcing stage, and thus facilitate the formation of a thin slag shell, thereby ensuring good surface quality of the bottom of the electroslag ingot.
[0026] (2) The present invention optimizes the physical and chemical properties of the slag system by optimizing the design of the slag system and rationally selecting the components of the slag system and their mass percentages; the slag system has a low melting point and viscosity, and is particularly suitable for electroslag remelting of high-temperature alloys with low melting points. At the same time, the stability of the slag system is controlled within a reasonable range, and the decomposition of the slag due to the reduction of the melting point and viscosity will not affect the remelting process. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 Schematic diagram of the structure of the electroslag remelting device in an embodiment of the present invention.
[0028] Figure 2 This is the high-temperature alloy electroslag ingot prepared in Example 1 of the present invention.
[0029] Figure 3 This is the high-temperature alloy electroslag ingot prepared in Comparative Example 1 of the present invention.
[0030] Figure 4 This is the high-temperature alloy electroslag ingot prepared in Comparative Example 2 of the present invention.
[0031] Figure 5 This is the high-temperature alloy electroslag ingot prepared in Comparative Example 3 of the present invention.
[0032] Description of labels:
[0033] 1. Lower crystallizer;
[0034] 2. Upper crystallizer;
[0035] 3. Bottom water tank;
[0036] 4. Consumable electrode;
[0037] 5. Protective cover;
[0038] 6. Feeding port. DETAILED DESCRIPTION
[0039] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0040] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0041] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0042] The electroslag ingots in the following embodiments and comparative examples are all made of N08810 high-temperature alloy electroslag ingots. In fact, they can also be adapted to prepare other high-temperature alloy electroslag ingots with a melting point between 1280 and 1400° C., such as Hastelloy C-276, Incoloy 825, and Incoloy625.
[0043] Regarding the explanation of the mass percentages in the embodiments and comparative examples: the mass percentages of the first component premelted slag and the second component premelted slag are both calculated as the mass percentages of the entire slag system. For example, the mass fraction of Al2O3 in the first component premelted slag is 5% to 10%, which means that the mass fraction of Al2O3 in the first component premelted slag is 5% to 10% relative to the mass percentage of the entire slag system composed of the first component premelted slag and the second component premelted slag.
[0044] Example 1
[0045] The preparation target of Example 1 is to prepare a N08810 high-temperature alloy electroslag ingot with a diameter of 400 mm. The melting point of the N08810 high-temperature alloy electroslag ingot is 1360°C.
[0046] The components of the first component pre-melted slag are as follows: cryolite 18%, Al2O3 10%, CaF2 15%, MgF2 10%, NaF2%, AlF3 1%; the melting point of the first component pre-melted slag is 1050°C.
[0047] The components of the second component pre-melted slag are as follows: Al2O3 10%, CaF2 5%, MgF2 20%, TiO22%, CaO 7%; the melting point of the second component pre-melted slag is 1240°C.
[0048] The overall slag system composed of the first component pre-melted slag and the second component pre-melted slag has the following components: cryolite 18%, Al2O3 20%, CaF2 20%, MgF2 30%, TiO22%, CaO 7%, NaF 2%, AlF3 1%; the melting point of the slag system is 1170°C, the viscosity is 0.20 Pa.s; the conductivity is 2.5S.cm -1 .
[0049] The process of preparing the first component pre-melted slag is as follows: the components of the first component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible, the melting temperature is heated to 1250°C, the heat preservation time is 3 hours, and then cooled and crushed into particles with a diameter of 5 mm to prepare the first component pre-melted slag.
[0050] The process of preparing the second component pre-melted slag is as follows: the components of the second component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible, the melting temperature is heated to 1300°C, the heat preservation time is 2 hours, and then cooled and crushed into particles with a diameter of 2 mm to prepare the second component pre-melted slag.
[0051] The first component pre-melted slag and the second component pre-melted slag are prepared, and then electroslag remelting is performed. The crystallizer used in the electroslag remelting process adopts a split design, such as Figure 1As shown, it includes a lower crystallizer 1 and an upper crystallizer 2, which are arranged along the axial direction of the consumable electrode 4. The upper crystallizer 2 and the lower crystallizer 1 are fixedly connected by screws to form an inner cavity of the crystallizer. The two have different cooling channels, and the height of the lower crystallizer 1 is 250 mm. Figure 1 The left side of the middle lower crystallizer 1, the upper crystallizer 2 and the bottom water tank 3 is a cooling water inlet, and the right side is a cooling water outlet.
[0052] like Figure 1 As shown, the upper crystallizer 2, the lower crystallizer 1, the bottom water tank 3, the consumable electrode 4, and the protective cover 5 are installed in place, and a feeding port 6 is opened on one side of the upper part of the protective cover 5. The slag enters the crystallizer from the feeding port 6. In the arcing and slagging stage, cooling water is introduced into the upper crystallizer 2, the lower crystallizer 1, and the bottom water tank 3; the temperature difference between the inlet and outlet cooling water of the upper crystallizer 2 is 10°C, and the outlet water temperature does not exceed 40°C; the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is 30°C, and the outlet water temperature does not exceed 70°C.
[0053] The specific process of electroslag remelting is as follows:
[0054] (1) The arc is started and the power is turned on. The control voltage is 25 V and the current is 3500 A. The first component pre-melted slag is added to the crystallizer for melting. The slag melting time is 60 min and the slag melting temperature does not exceed 1250 ° C. The electrode does not melt during the melting process.
[0055] (2) After the first component pre-melted slag is melted, the voltage is controlled to 30 V and the current is 5500 A, and the second component pre-melted slag is added to the crystallizer for melting. The slag melting time is 10 min;
[0056] (3) After the second component pre-melted slag is melted, the normal remelting stage is carried out. The control voltage is 30V and the current is 6000A. One hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is adjusted to 10°C, and the outlet water temperature does not exceed 40°C.
[0057] The subsequent operation is conventional electroslag remelting to obtain N08810 high-temperature alloy electroslag ingot.
[0058] Example 1 The electroslag ingot prepared is as follows Figure 2 As shown, the bottom surface is smooth and the slag thickness is only 2 to 4 mm, so it can enter the subsequent process without further grinding or cutting.
[0059] Comparative Example 1
[0060] The difference between this comparative example and Example 1 is that the specific process of electroslag remelting is different, and the other operations are basically the same.
[0061] The specific process of electroslag remelting is as follows:
[0062] (1) Arcing and power on, the control voltage is 30V, the current is 5000A, the first component pre-melted slag and the second component pre-melted slag are added to the crystallizer at the same time, the slag melting time is 70min, and the slag melting temperature does not exceed 1450℃;
[0063] (2) During the normal remelting stage, the control voltage is 30 V and the current is 7000 A. One hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is adjusted to 10°C, and the outlet water temperature does not exceed 40°C;
[0064] The subsequent operation is conventional electroslag remelting to obtain N08810 high-temperature alloy electroslag ingot.
[0065] The electroslag ingot prepared in Comparative Example 1 is as follows Figure 3 As shown, there are slag grooves on the bottom surface, which need to be further polished or cut off before entering the subsequent process. The thickness of the slag skin is 8 to 18 mm.
[0066] Comparative Example 2
[0067] This comparative example adopts the same overall slag system as that of Example 1, except that the slag system does not distinguish between the first component and the second component.
[0068] The process of preparing the pre-melted slag of the integral slag system is as follows: the components of the integral slag system are mixed evenly; the mixture is melted in a graphite crucible at a melting temperature of 1400° C. for 3 hours, and then cooled and crushed into particles with a diameter of 5 mm to prepare the pre-melted slag of the slag system.
[0069] The specific process of electroslag remelting is as follows:
[0070] (1) Start the arc and turn on the power. The control voltage is 30V and the current is 5500A. Add 1 / 2 of the total amount of pre-melted slag into the crystallizer. The slag melting time is 35min and the slag melting temperature does not exceed 1400℃.
[0071] (2) Add the remaining pre-melted slag into the crystallizer, and the slag melting time is 35 minutes;
[0072] (3) During the normal remelting stage, the control voltage is 30 V and the current is 7000 A. One hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is adjusted to 10°C, and the outlet water temperature does not exceed 40°C.
[0073] The subsequent operation is conventional electroslag remelting to obtain N08810 high-temperature alloy electroslag ingot.
[0074] Comparative Example 2 The electroslag ingot prepared is as follows Figure 4 As shown, the bottom is uneven and needs further grinding or cutting before entering the subsequent process. The thickness of the slag skin is 5 to 15 mm.
[0075] Comparative Example 3
[0076] The difference between this comparative example and Example 1 is that the first component and the second component are not pre-melted, and the other operations are basically the same, and a N08810 high-temperature alloy electroslag ingot is prepared.
[0077] Comparative Example 3 The electroslag ingot prepared is as follows Figure 5 As shown, there are slag grooves on the bottom surface and it is uneven, which requires further grinding or cutting before entering the subsequent process. The thickness of the slag skin is 8 to 20 mm.
[0078] Example 2
[0079] N08810 high-temperature alloy electroslag ingot is used as the preparation target of Example 2; the consumable electrode used is the same as that in Example 1.
[0080] The components of the first component pre-melted slag are as follows: cryolite 26%, Al2O3 10%, CaF2 10%, MgF2 10%, NaF3%, AlF3 1%; the melting point of the first component pre-melted slag is 980°C.
[0081] The second component pre-molten slag has the following components: Al2O3 5%, CaF2 10%, MgF2 10%, TiO2 10%, CaO 5%; the melting point of the second component pre-molten slag is 1220°C.
[0082] The components of the overall slag system composed of the first component pre-melted slag and the second component pre-melted slag are as follows: cryolite 26%, Al2O3 15%, CaF2 20%, MgF2 20%, TiO2 10%, CaO 5%, NaF 3%, AlF3 1%; the melting point of the slag system is 1150°C, the viscosity is 0.18 Pa.s; the conductivity is 3.0 S.cm -1 .
[0083] The process of preparing the first component pre-melted slag is as follows: the components of the first component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible at a melting temperature of 1200° C. for 2.5 hours, and then cooled and crushed into particles with a diameter of 10 mm to prepare the first component pre-melted slag.
[0084] The process of preparing the second component pre-melted slag is as follows: the components of the second component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible at a melting temperature of 1350° C. for 1.5 hours, and then cooled and crushed into particles with a diameter of 4 mm to prepare the second component pre-melted slag.
[0085] The first component pre-melted slag and the second component pre-melted slag are prepared, and then electroslag remelting is performed. The equipment used for electroslag remelting is basically the same as that in Example 1, except that the height of the lower crystallizer 1 is 300 mm. Before the arcing and slag-forming stage, cooling water is passed into the upper crystallizer 2, the lower crystallizer 1, and the bottom water tank 3; the temperature difference between the inlet and outlet cooling water of the upper crystallizer 2 is 15°C and the outlet water temperature does not exceed 40°C; the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is 35°C, and the outlet water temperature does not exceed 70°C.
[0086] The specific process of electroslag remelting is as follows:
[0087] (1) The arc is started and the control voltage is 28V and the current is 3000A. The first component pre-melted slag is added to the crystallizer for melting. The slag melting time is 45min and the slag melting temperature does not exceed 1250℃. The electrode does not melt during the melting process.
[0088] (2) After the first component pre-melted slag is melted, the voltage is controlled to 32V and the current is 5000A, and the second component pre-melted slag is added to the crystallizer for melting. The slag melting time is 15 minutes;
[0089] (3) After the second component pre-melted slag is melted, the voltage is controlled to 32V and the current is 6500A to carry out the normal remelting stage. One hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is adjusted to 15°C, and the outlet water temperature does not exceed 40°C.
[0090] The subsequent operation is conventional electroslag remelting to obtain N08810 high-temperature alloy electroslag ingot.
[0091] The electroslag ingot prepared in Example 2 has a smooth bottom surface without slag grooves, and can enter the subsequent process without further grinding or cutting. The slag skin thickness is 2 to 5 mm.
[0092] Example 3
[0093] N08810 high-temperature alloy electroslag ingot is used as the preparation target of Example 3; the consumable electrode used is the same as that in Example 1.
[0094] The components of the first component pre-melted slag are as follows: cryolite 18%, Al2O3 5%, CaF2 11%, MgF2 15%, NaF2%, AlF3 1%; the melting point of the first component pre-melted slag is 1080°C.
[0095] The second component pre-molten slag has the following components: Al2O3 15%, CaF2 11%, MgF2 5%, TiO2 7%, CaO 10%; the melting point of the second component pre-molten slag is 1280°C.
[0096] The overall slag system composed of the first component pre-melted slag and the second component pre-melted slag has the following components: cryolite 18%, Al2O3 20%, CaF2 22%, MgF2 20%, TiO2 7%, CaO 10%, NaF 2%, AlF3 1%; the melting point of the slag system is 1230°C, the viscosity is 0.22Pa.s, and the conductivity is 2.6S.cm -1 .
[0097] The process of preparing the first component pre-melted slag is as follows: the components of the first component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible at a melting temperature of 1300° C. for 2 hours, and then cooled and crushed into particles with a diameter of 15 mm to prepare the first component pre-melted slag.
[0098] The process of preparing the second component pre-melted slag is as follows: the components of the second component pre-melted slag are mixed evenly; the mixture is melted in a graphite crucible at a melting temperature of 1500° C. for 1 hour, and then cooled and crushed into particles with a diameter of 5 mm to prepare the second component pre-melted slag.
[0099] The equipment used for electroslag remelting is basically the same as that in Example 1. The difference between the equipment is that the height of the lower crystallizer 1 is 200 mm. Before the arcing and slag forming stage, cooling water is passed into the upper crystallizer 2, the lower crystallizer 1, and the bottom water tank 3; the temperature difference between the inlet and outlet cooling water of the upper crystallizer 2 is 20°C and the outlet water temperature does not exceed 40°C; the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is 40°C, and the outlet water temperature does not exceed 70°C.
[0100] The specific process of electroslag remelting is as follows:
[0101] (1) The arc is started and the control voltage is 22V, the current is 4000A, and the first component pre-melted slag is added to the crystallizer for melting; the slag melting time is 30min, and the slag melting temperature does not exceed 1250℃; the electrode does not melt during the melting process;
[0102] (2) After the first component pre-melted slag is melted, the voltage is controlled to 28V and the current is 6500A, and the second component pre-melted slag is added to the crystallizer for melting. The slag melting time is 20min;
[0103] (3) After the second component pre-melted slag is melted, the voltage is controlled to 31V and the current is 7000A to carry out the normal remelting stage. One hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer 1 is adjusted to 20°C, and the outlet water temperature does not exceed 40°C.
[0104] The subsequent operation is conventional electroslag remelting to obtain N08810 high-temperature alloy electroslag ingot.
[0105] The electroslag ingot prepared in Example 3 has a smooth bottom surface without slag grooves, and can enter the subsequent process without further grinding or cutting. The slag skin thickness is 3 to 6 mm.
[0106] Example 4
[0107] N08810 high-temperature alloy electroslag ingot is used as the preparation target of Example 4; the consumable electrode used is the same as that in Example 1.
[0108] The first component pre-melted slag has the following components: cryolite 21%, Al2O3 8%, CaF2 10%, MgF2 12%, NaF2%, AlF3 2%; the melting point of the first component pre-melted slag is 1040°C.
[0109] The second component pre-molten slag has the following components: Al2O38%, CaF2 20%, MgF2 10%, TiO2 2%, CaO 5%; the melting point of the second component pre-molten slag is 1210°C.
[0110] The components of the overall slag system composed of the first component pre-melted slag and the second component pre-melted slag are as follows: cryolite 21%, Al2O3 16%, CaF2 30%, MgF2 22%, TiO2 2%, CaO 5%, NaF 2%, AlF3 2%; the melting point of the slag system is 1160°C, the viscosity is 0.18 Pa.s, and the conductivity is 3.3S.cm -1 .
[0111] The process of preparing the first component pre-melted slag and the second component pre-melted slag is the same as that in Example 1.
[0112] The equipment used for electroslag remelting is the same as that in Example 1, and the specific process of cooling water temperature control and electroslag remelting is the same as that in Example 1, to obtain N08810 high-temperature alloy electroslag ingot.
[0113] The electroslag ingot prepared in Example 4 has a smooth bottom surface without slag grooves, and can enter the subsequent process without further grinding or cutting. The slag skin thickness is 4 to 7 mm.
[0114] Example 5
[0115] N08810 high-temperature alloy electroslag ingot is used as the preparation target of Example 5; the consumable electrode used is the same as that in Example 1.
[0116] The first component pre-melted slag has the following components: cryolite 20%, Al2O3 8%, CaF2 10%, MgF2 15%, NaF4%, AlF31%; the melting point of the first component pre-melted slag is 1000°C.
[0117] The second component pre-molten slag has the following components: Al2O3 7%, CaF2 15%, MgF2 5%, TiO2 10%, CaO 5%; the melting point of the second component pre-molten slag is 1200°C.
[0118] The components of the overall slag system composed of the first component pre-melted slag and the second component pre-melted slag are as follows: cryolite 20%, Al2O3 15%, CaF2 25%, MgF2 20%, TiO2 10%, CaO 5%, NaF 4%, AlF3 1%; the melting point of the slag system is 1160°C, the viscosity is 0.16 Pa.s, and the conductivity is 2.7S.cm -1 .
[0119] The process of preparing the first component pre-melted slag and the second component pre-melted slag is the same as that in Example 1.
[0120] The equipment used for electroslag remelting is the same as that in Example 1, and the specific process of cooling water temperature control and electroslag remelting is the same as that in Example 1, to obtain N08810 high-temperature alloy electroslag ingot. The electroslag ingot prepared in Example 5 has a smooth bottom surface without slag grooves, and can enter the subsequent process without further grinding or cutting, and the slag skin thickness is 2 to 5 mm.
Claims
1. A slag system for gas shielded electroslag remelting, characterized in that: The slag system comprises a first component pre-melted slag and a second component pre-melted slag, wherein, in terms of mass percentage of the entire slag system: The first component pre-melted slag includes the following components: cryolite 18%-26%, Al2O3 5%-10%, CaF2 10%-15%, MgF2 10%-15%, NaF 2-4%, AlF3 1-2%; the melting point of the first component pre-melted slag is 960-1100°C; The second component pre-melted slag includes the following components: Al2O3 5% to 15%, CaF2 5% to 20%, MgF2 5% to 20%, TiO2 2% to 10%, CaO 5% to 10%; the melting point of the second component pre-melted slag is 1200 to 1300°C; The first component pre-melted slag and the second component pre-melted slag are used to be added into the crystallizer in batches during the arcing and slagging stage.
2. The slag system for gas-shielded electroslag remelting according to claim 1, characterized in that: The overall slag system composed of the first component pre-melted slag and the second component pre-melted slag includes the following components in mass percentage: cryolite 18%-26%, Al2O3 15-20%, TiO2 2%-10%, CaF2 20%-30%, MgF2 20%-30%, CaO 5%-10%, NaF2-4%, and AlF3 1-2%.
3. The slag system for gas-shielded electroslag remelting according to claim 2, characterized in that: The melting point of the slag system is 1150-1250°C, the viscosity is 0.12-0.24 Pa.s, and the conductivity is 2.5-3.5 S.cm -1 , the stability is 1.69~1.
75.
4. The slag system for gas shielded electroslag remelting according to any one of claims 1 to 3, characterized in that: The particle sizes of the first component pre-melted slag and the second component pre-melted slag are 5-15 mm and 2-5 mm respectively.
5. A method for preparing a slag system for gas shielded electroslag remelting according to any one of claims 1 to 4, characterized in that: include: The mixed materials of the components of the first component pre-melted slag are heated and melted, and then cooled and crushed to obtain the first component pre-melted slag; The mixed materials of the components of the second component pre-melted slag are heated and melted, and then cooled and crushed to obtain the second component pre-melted slag.
6. The method for preparing a slag system for gas-shielded electroslag remelting according to claim 5, characterized in that: The heating and melting temperature of the first component pre-melted slag is 1200-1300°C, and the heating and melting temperature of the second component pre-melted slag is 1300-1500°C.
7. A method for using the slag system for gas shielded electroslag remelting according to any one of claims 1 to 4, characterized in that: include: (1) Arcing and powering on; the control voltage is 22-28V, the current is 3000-4000A, and the first component pre-melted slag is first added into the crystallizer for melting, and the slag melting temperature does not exceed 1250°C; (2) After the first component pre-melted slag is melted, the voltage is controlled to be 28-32V and the current is 5000-6500A, and then the second component pre-melted slag is added to the crystallizer for melting; (3) After the second component pre-molten slag is melted, the voltage is controlled to 30-32V and the current is 6000-7000A to carry out the normal remelting stage.
8. The method for using the slag system for gas-shielded electroslag remelting according to claim 7, characterized in that: The melting time of the first component pre-melted slag is 30 to 60 minutes.
9. The method for using the slag system for gas-shielded electroslag remelting according to claim 7, characterized in that: The melting time of the second component pre-melted slag is 10 to 20 minutes.
10. The method for using the slag system for gas shielded electroslag remelting according to any one of claims 7 to 9, characterized in that: The crystallizer comprises a lower crystallizer (1) and an upper crystallizer (2), both of which are arranged along the axial direction of the consumable electrode (4), and the height of the lower crystallizer (2) is 200-300 mm; in the arcing and slag-melting stage, the temperature difference between the inlet and outlet cooling water of the upper crystallizer (2) is 10-20°C and the outlet water temperature does not exceed 40°C, and the temperature difference between the inlet and outlet cooling water of the lower crystallizer (1) is 30-40°C and the outlet water temperature does not exceed 70°C; one hour after entering the normal remelting stage, the temperature difference between the inlet and outlet cooling water of the lower crystallizer (1) is adjusted to 10-20°C and the outlet water temperature does not exceed 40°C.