Large-specification multi-layer composite aluminum foil and preparation method thereof

By optimizing the rolling, slitting and annealing process of aluminum foil, the problems of hot and cold stress and oil removal difficulties of film cabin materials are solved, and the efficient preparation of aluminum foil is achieved, which improves the safety and efficiency of liquefied natural gas storage and transportation.

CN119082558AInactive Publication Date: 2024-12-06CHINALCO HENAN LUOYANG ALUMINUM FOIL CO LTD +1

Patent Information

Application Number
CN202411571770.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing film cabin enclosure system materials have limitations in terms of hot and cold stress, which are prone to deformation or damage, which affects the efficiency and safety of liquefied natural gas storage and transportation. It is difficult to completely remove the rolling oil in the slitting process, affecting the aluminum foil Mechanical performance and production efficiency.

Method used

A large-scale multi-layer composite aluminum foil and its preparation method were developed. By optimizing the rolling, slitting and annealing process, the volatility and oil removal process of the rolling oil is controlled to ensure that the oil is completely removed and the formation of oil spots is avoided, while improving the Mechanical properties and production efficiency of aluminum foil. Specific steps include foil rolling, slitting and multi-stage precisely controlled annealing process, including stress relief, low-temperature oil removal, performance improvement and high-temperature oil removal stages to ensure the surface of the aluminum foil is clean and the mechanical properties are optimized.

Benefits of technology

It effectively improves production efficiency, reduces the amount of residual oil on the surface of the aluminum foil, ensures the mechanical properties and barrier properties of the aluminum foil, avoids the formation of oil spots and secondary pollution, and improves the performance of thin-film cabin materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082558A_ABST
    Figure CN119082558A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of non-ferrous metal processing, and particularly discloses a large-size multi-layer composite aluminum foil and a preparation method thereof.The aluminum foil comprises, by weight, 0.07%-0.25% of Si, 0.035%-0.50% of Fe, 0.0005%-0.02% of Cu and the balance Al and other added elements, and the sum of the weight of the other added elements is smaller than or equal to 0.040%. The preparation method of the aluminum foil specifically comprises the steps of foil rolling, slitting and annealing. A set of suitable rolling, slitting and annealing process is developed, the production efficiency is effectively improved on the basis that rolling oil is fully volatilized, and through the multi-section accurate control oil removal annealing process, on one hand, the oil removal temperature is increased, the oil removal time is prolonged, on the basis that it is guaranteed that the oil is not excessively burnt, the oil in the core of a coil material is completely removed, and the production cost is reduced. Oil spots can be prevented from being formed on the surface of the aluminum foil, and meanwhile adverse effects on the mechanical property of an aluminum foil coil stock finished product can be avoided; on the other hand, the distance between the roll materials is increased, and secondary pollution caused by volatile oil products is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metal processing, in particular to a large-size multi-layer composite aluminum foil and a preparation method thereof. Background Art

[0002] At present, aluminum foil widely used under industrial conditions is divided into hard and soft states. The main difference is that soft aluminum foil needs to have good forming properties for subsequent processing operations. Because aluminum foil is relatively soft, industrial aluminum foil is rarely used alone. It is generally required to be used in combination with paper, polymer resin materials, glass fiber cloth, etc. to form a multi-layer composite material. As the core material of the multi-layer composite material, aluminum foil needs to have good forming properties, barrier properties and temperature resistance. It is widely used in the fields of LNG ship low-temperature containment system, new energy lithium battery packaging, pharmaceutical packaging and food packaging to ensure the safety and stability of the packaged objects. This kind of aluminum foil is usually made of 8xxx aluminum alloy, the main components of which are Fe and Si elements and other trace elements.

[0003] Taking the aluminum foil of the shielding layer of the liquefied natural gas maintenance system as an example, through advanced compression and cooling technology, natural gas can be converted into liquid at a low temperature of about -161.5℃, which facilitates efficient storage and transportation under conditions close to -161.5℃ and 0.1MPa.

[0004] LNG membrane cabins play a vital role in the storage and transportation of liquefied natural gas. This specially designed cabin not only needs to have excellent sealing to prevent gas leakage, but also excellent insulation performance to maintain a stable low-temperature environment. Among them, the shielding layer, as a key component of the LNG containment system in the cabin, is composed of aluminum foil and glass fiber cloth. It is divided into a rigid sub-shielding layer and a flexible sub-shielding layer, which provides a strong barrier and insulation effect for the containment system. The surface roughness and mechanical properties of the aluminum foil have a decisive influence on the quality and performance of the shielding layer.

[0005] With the continuous growth of my country's economy and the increasing awareness of environmental protection, the application and development of liquefied natural gas is attracting more and more attention from all parties. However, the current membrane materials of membrane gas storage tanks still have certain limitations in dealing with cold and hot stresses, and are prone to deformation or damage, which to a certain extent restricts the further development and promotion of LNG storage technology. Therefore, improving the performance of membrane-type cabin enclosure system materials has become the key to promoting the sustainable and healthy development of the liquefied natural gas industry.

[0006] The slitting process is a key process in the production of aluminum foil. The influence of slitting process parameters on the residual oil on the surface of aluminum foil after annealing cannot be ignored, especially for aluminum foil coils with wider width after slitting. The closer to the core of the coil, the more difficult it is to remove the residual oil on the surface. Usually, the degreasing annealing time or the annealing temperature is increased to remove the oil. However, when the annealing temperature is too high or the heating rate is too fast, the rolling oil may burn excessively, producing a large amount of smoke and harmful gases. At the same time, it will also form oil spots on the surface of the aluminum foil that are difficult to remove. The annealing process will seriously affect the mechanical properties of the finished aluminum foil coil, and increasing the annealing time will greatly reduce the production efficiency, resulting in greater difficulty in producing aluminum foil with good wetting properties.

[0007] Therefore, the present invention provides a large-size multi-layer composite aluminum foil and a preparation method thereof to solve the above-mentioned problems. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the existing defects, provide a large-size multi-layer composite aluminum foil and a preparation method thereof, develop a set of suitable rolling, slitting and annealing processes, and effectively improve the production efficiency on the basis of fully volatilizing the rolling oil. In addition, the degreasing annealing process is precisely controlled in multiple stages. On the one hand, the degreasing temperature and time are increased, and the oil in the core of the coil is completely removed while ensuring that the oil is not excessively burned, which can avoid the formation of oil spots on the surface of the aluminum foil and avoid adverse effects on the mechanical properties of the finished aluminum foil coil. On the other hand, the spacing between the coils is increased to prevent secondary pollution caused by volatile oil, which can effectively solve the problems in the background technology.

[0009] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a large-scale LNG containment system shielding layer aluminum foil, whose components, calculated by weight percentage, include: Si: 0.07-0.25%, Fe: 0.035-0.50%, Cu: 0.0005-0.02%, and the remainder is Al and other added elements, and the sum of the weights of other added elements is ≤0.040%.

[0010] A method for preparing a large-scale LNG containment system shielding layer aluminum foil comprises the following steps: S1. Foil rolling: rolling the aluminum foil blank with a thickness of 0.2-0.4 mm to the aluminum foil finished product with a thickness of 50-100 μm, with a rolling rate of 285-400 m / min and a roller roughness of 0.1-0.15 μm; S2. Slitting: Cut the finished aluminum foil roll into small aluminum foil rolls with a width of 700-1200mm using a slitting machine, with a slitting tension of 5-10MPa and a support roller pressure of 0.5-1.0Mpa; S3, Annealing: Annealing includes the following 4 stages: During the stress release stage, the temperature is raised to 50-90°C at a rate of 5-15°C / h and kept at this temperature for 3-6h; In the low-temperature degreasing stage, the temperature is raised to 200-220°C at a rate of 15-20°C / h and kept at this temperature for 20-25h; In the performance improvement stage, the temperature is raised to 220-270°C at a rate of 15-30°C / h and kept at this temperature for 5-10h; In the high-temperature degreasing stage, the temperature is raised to 400-420°C at a rate of 10-20°C / h and kept at this temperature for 60-75h; After annealing, the steel is cooled at a rate of 2-10°C / h to below 90°C, kept at this temperature for 5-10h, and then taken out of the furnace and air-cooled.

[0011] As a preferred technical solution of the present invention, in S1 foil rolling, rolling oil is added during rolling, and the rolling oil is a mixture of base oil and acid and alcohol additives.

[0012] As a preferred technical solution of the present invention, during the S3 annealing process, the distance between the aluminum foil rolls is ≥35 cm.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention exemplifies a large-size multi-layer composite aluminum foil and a preparation method thereof. Based on the thickness and width of the aluminum foil, the present invention develops a set of suitable rolling, slitting and annealing processes, which effectively improves production efficiency while fully volatilizing the rolling oil.

[0014] The large-size multi-layer composite aluminum foil and its preparation method exemplified in the present invention reduce the non-volatile components in the rolling oil and the oil throwout during the rolling process by controlling the rolling rate and the composition of the rolling oil, thereby effectively controlling the amount of oil on the surface of the aluminum foil coil and reducing the difficulty of subsequent oil removal.

[0015] The large-size multi-layer composite aluminum foil and its preparation method exemplified in the present invention accurately control the degreasing annealing process in multiple stages. On the one hand, the degreasing temperature and time are increased to completely remove the oil in the core of the coil while ensuring that the oil is not over-burned; on the other hand, the spacing between the coils is increased to prevent secondary pollution caused by volatile oil. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a process flow chart of the present invention; Figure 2 This is a macroscopic picture of the aluminum foil sample 1 in the present invention; Figure 3 This is a microscopic picture of the aluminum foil sample 1 in the present invention; Figure 4 This is a macroscopic picture of the aluminum foil sample 2 in the present invention; Figure 5This is a microscopic picture of the aluminum foil sample 2 in the present invention; Figure 6 This is a macroscopic picture of the aluminum foil sample 3 in the present invention; Figure 7 This is a microscopic picture of the aluminum foil sample 3 in the present invention; Figure 8 The following is a macroscopic picture of the comparison of aluminum foil samples with oil spots.

[0017] Fig. 9 The following is a microscopic picture of the comparison of aluminum foil samples with oil spots. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Embodiment 1:

[0019] A large-size multi-layer composite aluminum foil comprises, by weight percentage, 0.07% Si, 0.035% Fe, 0.0005% Cu, and the remainder Al and other additive elements, wherein the sum of the weights of the other additive elements is 0.040%.

[0020] like Figure 1 As shown, the preparation method of the large-size multi-layer composite aluminum foil comprises the following steps: S1. Foil rolling: rolling the aluminum foil blank with a thickness of 0.4 mm to the finished aluminum foil with a thickness of 50 μm, with a rolling rate of 400 m / min and a roller roughness of 0.15 μm; adding rolling oil during rolling, the rolling oil is a mixture of base oil and acid and alcohol additives, wherein the base oil is 70# or 80# kerosene, and the additives are mainly lauric acid and lauric alcohol, such as lauric acid and lauric alcohol, and the total ratio of the two is 3-5% of the total volume of the rolling oil.

[0021] S2. Slitting: The finished aluminum foil roll is cut into small aluminum foil rolls with a width of 700 mm by a slitting machine, with a slitting tension of 5 MPa and a support roller pressure of 0.5 MPa; S3, Annealing: Annealing includes the following 4 stages: In the stress release stage, the temperature was raised to 50°C at a rate of 15°C / h and kept at this temperature for 3h; In the low-temperature degreasing stage, the temperature is raised to 200°C at a rate of 20°C / h and kept at this temperature for 20h; In the performance improvement stage, the temperature was raised to 220°C at a rate of 30°C / h and kept at this temperature for 5h; In the high-temperature degreasing stage, the temperature is raised to 400°C at a rate of 20°C / h and kept at this temperature for 60h; After annealing, the aluminum foil is cooled at a rate of 10°C / h to below 90°C. After keeping warm for 5 hours, it is taken out of the furnace and air-cooled. In addition, during the annealing process, the distance between the aluminum foil rolls is ≥35cm.

[0022] Aluminum foil sample 1 prepared according to the above preparation method. Embodiment 2:

[0023] A large-size multi-layer composite aluminum foil comprises, by weight percentage, 0.25% Si, 0.1% Fe, 0.02% Cu, and the remainder Al and other additive elements, wherein the sum of the weights of the other additive elements is 0.030%.

[0024] like Figure 1 As shown, the preparation method of the large-size multi-layer composite aluminum foil comprises the following steps: S1. Foil rolling: rolling the aluminum foil blank with a thickness of 0.3 mm to the finished aluminum foil with a thickness of 80 μm, with a rolling rate of 350 m / min and a roller roughness of 0.1 μm; adding rolling oil during rolling, the rolling oil is a mixture of base oil and acid and alcohol additives, wherein the base oil is 70# or 80# kerosene, and the additives are mainly lauric acid and lauric alcohol, such as lauric acid and lauric alcohol, and the total ratio of the two is 3-5% of the total volume of the rolling oil.

[0025] S2. Slitting: The finished aluminum foil roll is cut into small aluminum foil rolls with a width of 900 mm by a slitting machine, with a slitting tension of 7 MPa and a support roller pressure of 1.0 MPa; S3, Annealing: Annealing includes the following 4 stages: In the stress release stage, the temperature was raised to 75°C at a rate of 10°C / h and kept at this temperature for 5h; In the low-temperature degreasing stage, the temperature was raised to 210°C at a rate of 18°C / h and kept at this temperature for 22h; In the performance improvement stage, the temperature was raised to 250°C at a rate of 20°C / h and kept at this temperature for 8h; In the high-temperature degreasing stage, the temperature was raised to 410°C at a rate of 15°C / h and kept at that temperature for 70h; After annealing, the aluminum foil is cooled at a rate of 8°C / h to below 90°C. After keeping warm for 8 hours, it is taken out of the furnace and air-cooled. In addition, during the annealing process, the distance between the aluminum foil coils is ≥35cm.

[0026] Aluminum foil sample 2 prepared according to the above preparation method. Embodiment three:

[0027] A large-size multi-layer composite aluminum foil comprises, by weight percentage, 0.1% Si, 0.50% Fe, 0.01% Cu, and the remainder Al and other added elements, wherein the sum of the weights of the other added elements is 0.020%.

[0028] like Figure 1 As shown, the preparation method of the large-size multi-layer composite aluminum foil comprises the following steps: S1. Foil rolling: rolling the aluminum foil blank with a thickness of 0.2 mm to the finished aluminum foil with a thickness of 100 μm, with a rolling rate of 325 m / min and a roller roughness of 0.12 μm; adding rolling oil during rolling, the rolling oil is a mixture of base oil and acid and alcohol additives, wherein the base oil is 70# or 80# kerosene, and the additives are mainly lauric acid and lauric alcohol, such as lauric acid and lauric alcohol, and the total ratio of the two is 3-5% of the total volume of the rolling oil.

[0029] S2. Slitting: The finished aluminum foil roll is cut into small aluminum foil rolls with a width of 1100 mm by a slitting machine, with a slitting tension of 10 MPa and a support roller pressure of 0.8 MPa; S3, Annealing: Annealing includes the following 4 stages: In the stress release stage, the temperature was raised to 90°C at a rate of 5°C / h and kept at this temperature for 6h; In the low-temperature degreasing stage, the temperature was raised to 220°C at a rate of 15°C / h and kept at this temperature for 25h; In the performance improvement stage, the temperature was raised to 270°C at a rate of 15°C / h and kept at this temperature for 10h; In the high-temperature degreasing stage, the temperature was raised to 420°C at a rate of 10°C / h and kept at that temperature for 75h; After annealing, the aluminum foil is cooled at a rate of 2°C / h to below 90°C. After keeping warm for 10 hours, it is taken out of the furnace and air-cooled. In addition, during the annealing process, the distance between the aluminum foil coils is ≥35cm.

[0030] Other elements in Examples 1 to 3 include Cr, V, Ti, and Ca.

[0031] Aluminum foil sample three prepared according to the above preparation method.

[0032] The performance parameters of aluminum foil sample 1, aluminum foil sample 2, and aluminum foil sample 3 are shown in the following table:

[0033] Figure 2 This is a macroscopic picture of aluminum foil sample 1. Figure 3 This is a microscopic picture of aluminum foil sample 1; Figure 4 This is a macro picture of aluminum foil sample 2. Figure 5 This is a microscopic picture of aluminum foil sample 2; Figure 6 This is a macro picture of aluminum foil sample 3. Figure 7 This is a microscopic picture of aluminum foil sample 3; Figure 8 This is a macroscopic picture of aluminum foil with oil spots in the prior art. Fig. 9 This is a microscopic picture of aluminum foil with oil spots in the prior art.

[0034] The present invention develops a set of suitable rolling, slitting and annealing processes based on the thickness and width of the aluminum foil, which effectively improves the production efficiency on the basis of fully volatilizing the rolling oil; and the present invention reduces the components that are difficult to volatilize in the rolling oil and reduces the oil throwing out during the rolling process by controlling the rolling rate and the composition of the rolling oil, thereby effectively controlling the amount of oil on the surface of the aluminum foil coil and reducing the difficulty of subsequent oil removal; the present invention accurately controls the oil removal annealing process through multiple stages, on the one hand, increases the oil removal temperature and time, and completely removes the oil in the core of the coil while ensuring that the oil is not over-burned; on the other hand, increases the spacing between the coils to prevent secondary pollution caused by volatile oil.

[0035] In the present invention, firstly, the influence of rolling oil components, slitting process and annealing process of double-sided smooth aluminum foil on the residual oil on the surface of aluminum foil coil after annealing is a complex and delicate process, involving key technologies of multiple processes of aluminum foil production. Firstly, the influence of slitting process parameters on the residual oil on the surface of aluminum foil coil after annealing cannot be ignored, and slitting process is a key process in the production process of aluminum foil. For aluminum foil coils with a finished width of 700-1100mm, due to its narrow width, annealing and oil removal are more difficult, especially it is very difficult to completely remove the grease in the core of the coil layer. Therefore, it is necessary to control during the rolling process. The faster the rolling rate, the more oil will be thrown out and adhere to the surface of the aluminum foil, which will affect the subsequent oil removal process. Therefore, the rolling rate is controlled at a lower state to lay the foundation for subsequent thorough oil removal. At the same time, the components of the rolling oil will directly affect the amount of oil on the aluminum foil; if the rolling oil contains more impurities or additives, these substances are more likely to remain on the surface of the aluminum foil during the rolling process, forming oil spots that are difficult to remove. Therefore, the amount of acid and alcohol added to the rolling oil is controlled between 3-5%, and the addition of ester is limited. While ensuring the strength of the oil film during the rolling process, the thickness of the oil film is effectively controlled to improve the volatilization efficiency of the oil during the annealing process.

[0036] Secondly, during the slitting process, the support roller pressure, slitting tension, etc. will directly affect the porosity of the small coil after slitting, thereby affecting the volatilization efficiency of the oil during the annealing process, and further determining the degreasing effect. In the present invention, the slitting tension is controlled at 5-10MPa and the support roller pressure is 0.5-1.0MPa, so that the porosity of the small coil after slitting is controlled between 12-15%, which is conducive to the full volatilization of the rolling oil in the core of the coil from the gap, while ensuring that the small coil after slitting does not have staggered layers and tower-shaped defects.

[0037] Finally, in the degreasing annealing process, the annealing temperature, time, and heating / cooling rate will directly affect the residual oil and wetting tension on the surface of the aluminum foil coil after annealing, and will also affect the internal stress and ductility of the aluminum foil. For aluminum foil coils with a wider width, high-temperature annealing is required to improve production efficiency. However, if the annealing temperature is too high, excessive combustion of rolling oil is likely to occur, generating a large amount of smoke and harmful gases. At the same time, oil spots that are difficult to remove will also form on the surface of the aluminum foil. On the other hand, the mechanical properties of the aluminum foil will be significantly reduced, affecting its use. Therefore, the low-temperature degreasing stage is controlled, and the temperature is increased to 200-220℃ at a rate of 15-20℃ / h, and the temperature is kept for 20-25h; in the high-temperature degreasing stage, the temperature is increased to 400-420℃ at a rate of 10-20℃ / h, and the temperature is kept for 60-75h. The slow heating method is used to preheat the oil to prevent excessive combustion, and the high-temperature degreasing temperature and insulation time are increased to ensure that the oil in the core of the coil is completely volatilized. On the other hand, the distance between each coil is expanded to more than 35 cm in order to prevent the oil volatilized between each coil from contaminating other coils again.

[0038] The present invention comprehensively considers the requirements of mechanical properties and surface wetting tension, reasonably sets the heating rate, holding temperature and temperature time, and controls the atmosphere and time in the annealing process under the premise of ensuring production efficiency, so as to reduce the residual oil on the surface of the aluminum foil coil after annealing.

[0039] The undisclosed parts in the present invention are all prior art, and their specific structures, materials and working principles are not described in detail. Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the attached claims and their equivalents.

Claims

1. A large-size multi-layer composite aluminum foil, characterized in that: The ingredients are calculated by weight percentage Including: Si: 0.07-0.25%, Fe: 0.035-0.50%, Cu: 0.0005-0.02%, the balance is Al and other added elements, and the sum of the weight of other added elements is ≤0.040%.

2. A method for preparing a large-size multi-layer composite aluminum foil according to claim 1, characterized in that: The following steps are involved: S1. Foil rolling: rolling the aluminum foil blank with a thickness of 0.2-0.4 mm to the aluminum foil finished product with a thickness of 50-100 μm, with a rolling rate of 285-400 m / min and a roller roughness of 0.1-0.15 μm; S2. Slitting: Cut the finished aluminum foil roll into small aluminum foil rolls with a width of 700-1200mm using a slitting machine, with a slitting tension of 5-10MPa and a support roller pressure of 0.5-1.0Mpa; S3, Annealing: Annealing includes the following 4 stages: During the stress release stage, the temperature is raised to 50-90°C at a rate of 5-15°C / h and kept at this temperature for 3-6h; In the low-temperature degreasing stage, the temperature is raised to 200-220°C at a rate of 15-20°C / h and kept at this temperature for 20-25h; In the performance improvement stage, the temperature is raised to 220-270°C at a rate of 15-30°C / h and kept at this temperature for 5-10h; In the high-temperature degreasing stage, the temperature is raised to 400-420°C at a rate of 10-20°C / h and kept at this temperature for 60-75h; After annealing, the steel is cooled at a rate of 2-10°C / h to below 90°C, kept at this temperature for 5-10h, and then taken out of the furnace and air-cooled.

3. The method for preparing a large-size multi-layer composite aluminum foil according to claim 2, characterized in that: During S1 foil rolling, rolling oil is added during rolling, and the rolling oil is a mixture of base oil and acid and alcohol additives.

4. The method for preparing a large-size multi-layer composite aluminum foil according to claim 2, characterized in that: During the S3 annealing process, the distance between aluminum foil rolls is ≥35cm.

Citation Information

Patent Citations

  • Method for producing aluminum alloy medicinal foil by hot-rolling method

    CN101338392A

  • Aluminum foil material capable of meeting more than 4 mm punching depth of cold punch formed flexible package material

    CN102329984A

  • Aluminum foil suitable for solar flat-plate heat collector, and production method thereof

    CN103484725A

  • Aluminum roll annealing and oil-removing method

    CN110195197A

  • Low-pinhole thin aluminum foil for flexible packages and production process thereof

    CN110423920A

Cited By

  • LNG containment system shielding layer aluminum foil and preparation method thereof

    CN119657636A

  • Aluminum foil for 0.05 mm lamp strip label and preparation method of aluminum foil

    CN120738523A