High-Mn type Mn-Cu-based high-damping alloy and preparation method thereof
The high-Mn Mn-Cu alloy with specific compositions and enhanced processing methods addresses the low phase transition and narrow temperature range issues, offering improved damping performance across a broader temperature range.
Patent Information
- Application Number
- CN202411221846.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
Existing Mn-Cu alloys have a low phase transition temperature and a narrow applicable temperature range, limiting their stability and effectiveness in damping performance across various ambient temperatures.
A high-Mn type Mn-Cu based alloy with specific compositions (22.5-26.5% Cu, 1-2% Al, 0.8-1.2% Sn, balance Mn) and a two-stage smelting, casting, forging, and heat treatment process to enhance phase transition temperature and stability.
The alloy exhibits improved phase transition temperature and damping performance across a wider temperature range, suitable for practical applications under varying conditions.
Smart Images

Figure CN119082569A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high damping alloys, and in particular to a high-Mn type Mn-Cu based high damping alloy and a preparation method thereof. Background Art
[0002] With the development of society, science and technology around the world are gradually becoming more developed. The advanced level of science and technology has greatly improved people's material living standards. However, with the emergence of modern scientific and technological products such as new buildings, ships, and high-speed railways, the adverse effects of vibration and noise on humans and the environment are gradually increasing. Therefore, it is particularly important to develop efficient vibration reduction and noise reduction technologies and materials. At present, there are three main means to achieve the purpose of reducing vibration and noise. First, by using more solid workpieces to achieve the goal of reducing vibration; second, by adding sound insulation devices to engineering machinery and equipment; third, by using efficient and environmentally friendly damping materials to suppress noise from the source. Even if the first two methods can effectively control vibration and noise, there are still disadvantages of making mechanical equipment heavier, larger, and more expensive. The use of damping materials can effectively reduce harmful vibration and noise from the source.
[0003] Mn-Cu alloy is a typical high damping alloy with excellent damping performance and mechanical properties, so it is widely used in the field of vibration and noise control. The damping mechanism of Mn-Cu alloy comes from the relaxation movement of its internal twin boundaries and phase boundaries when affected by external energy, thereby dissipating the external energy. When the supersaturated solid solution Mn-Cu alloy is aged within the metastable miscible temperature range, spinodal decomposition will occur inside the alloy. A large number of nano-scale Mn-rich and Cu-rich regions are generated inside the alloy through spinodal decomposition. The Mn content in the Mn-rich region is an important factor affecting the damping performance of the alloy. The higher the Mn content in the Mn-rich region, the higher the FCC-FCT phase transition point of the alloy will be, so it is more conducive to the formation of the FCT phase. The energy dissipation brought by the movement of more FCT phase boundaries improves the damping performance of the alloy. In addition, when the phase change occurs, a large number of martensitic twins and (110) twin boundaries are induced, and the energy obtained from the outside is dissipated through the movement of twin boundaries and phase boundaries, so that the Mn-Cu alloy has extremely excellent damping properties.
[0004] The phase transition temperature of general Mn-Cu based damping alloys is near room temperature, but the damping performance will decay sharply under conditions slightly above room temperature, which greatly limits the applicable temperature range of Mn-Cu alloys. At present, there is still a lack of methods to enable Mn-Cu to be stably applied in a wider and higher temperature range. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a high-Mn type Mn-Cu based high damping alloy and a preparation method thereof, so as to solve the problems that the existing Mn-Cu alloy has a low phase transition temperature, a small applicable temperature range of damping performance, and is difficult to be stably applied in a wider and higher temperature range.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] A high-Mn type Mn-Cu based high damping alloy comprises the following raw materials in mass percentage: 22.5-26.5% Cu, 1-2% Al and 0.8-1.2% Sn, with the balance being Mn.
[0008] The beneficial effects of the present invention are as follows: the present invention provides a formula of a high-Mn type Mn-Cu based high damping alloy, which increases the phase transition temperature of the alloy by increasing the Mn content in the alloy and the method of doping Sn, thereby promoting the formation of more martensitic structures on the one hand, and expanding the temperature range with excellent damping performance through the martensite with higher stability during the heating process on the other hand, thereby solving the technical problem in the prior art that the applicable temperature range of Mn-Cu alloy is narrow and it is difficult to carry out practical application under various ambient temperatures.
[0009] Further, the raw materials include the following mass percentages: Cu 22.5%, Al 1.5% and Sn 1%, and the balance is Mn; or Cu 24.5%, Al 1.5% and Sn 1%, and the balance is Mn; or Cu 26.5%, Al 1.5% and Sn 1%, and the balance is Mn.
[0010] The preparation method of the above-mentioned high-Mn type Mn-Cu based high damping alloy comprises the following steps:
[0011] The raw materials are first mixed and smelted, and then rare gas is added to continue smelting, and then cast to obtain an alloy ingot, and finally the obtained alloy ingot is annealed, forged and heat treated to obtain the alloy.
[0012] The beneficial effects of the present invention are as follows: the present invention is prepared by casting + forging, the preparation method is simple and easy to implement, and different from the traditional casting method, the present invention further ensures the stability of the high Mn type Mn-Cu alloy through a high temperature forging process and increases the phase change temperature.
[0013] Furthermore, the smelting power is 28-32 kW, and the smelting is performed until the raw materials are completely melted.
[0014] Preferably, the smelting power is 30 kW, and the smelting is carried out until the raw materials are completely melted.
[0015] Further, rare gas is charged until the pressure reaches 0.05-0.07Mpa, and the smelting power is continued at 18-22kW until the raw materials are evenly mixed.
[0016] Preferably, rare gas is charged until the pressure reaches 0.06 MPa, the smelting power is continued at 20 kW, and the smelting is continued until the raw materials are evenly mixed.
[0017] The beneficial effect of adopting the above technical solution is as follows: the present invention adopts a two-stage smelting method, which ensures the complete melting of the raw materials during the smelting process, avoids the occurrence of small impurities that are not completely melted, and ensures the uniformity of the raw material mixing, thereby ensuring the uniformity of the alloy components subsequently obtained.
[0018] Furthermore, the annealing conditions are: keeping at 800-900° C. for 20-30 hours and then air cooling to room temperature.
[0019] Preferably, the annealing condition is: keeping at 850° C. for 24 hours and then air cooling to room temperature.
[0020] Furthermore, the starting forging temperature of the forging is 800-900°C, and the ending forging temperature is 600-650°C.
[0021] Preferably, the starting forging temperature of forging is 850°C and the ending forging temperature is 620°C.
[0022] Furthermore, the heat treatment conditions are: first keep at 850-900°C for 0.5-2h and then air cool to room temperature, then keep at 350-380°C for 1-3h and then air cool to room temperature to complete the heat treatment.
[0023] Preferably, the heat treatment conditions are: first keep at 880°C for 1 hour and then air cool to room temperature, then keep at 360°C for 2 hours and then air cool to room temperature to complete the heat treatment.
[0024] The beneficial effect of adopting the above further technical solution is: the present invention anneals and heat treats the alloy ingots before and after forging, and improves and optimizes the heat treatment conditions, thereby effectively improving the uniformity of the structure and composition of the obtained alloy, and improving the strength and damping performance of the alloy.
[0025] The above high Mn type Mn-Cu based high damping alloy is used in reducing vibration and noise in industry.
[0026] The present invention has the following beneficial effects:
[0027] (1) The preparation method of the high-Mn type Mn-Cu high damping alloy of the present invention is simple and low in cost; different from the common research on M2052 type alloy, the present invention increases the Mn content while also performing a high-temperature forging process, and the alloy forging process is more in line with the conditions in actual engineering applications.
[0028] (2) The phase transition temperature of the high-Mn type Mn-Cu high damping alloy of the present invention can be controlled by adjusting the Mn / Cu atomic ratio. The prepared alloy has a higher phase transition temperature, which can promote the formation of more martensite on the one hand, and on the other hand, the martensite has better stability during the heating process, so that it can have better damping performance within a certain temperature range. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The damping strain amplitude curve diagram of the high-Mn type Mn-Cu high damping alloy obtained in Example 1;
[0030] Figure 2 The temperature-damping curve of the high-Mn type Mn-Cu high-damping alloy obtained in Example 1;
[0031] Figure 3 The temperature-modulus curve of the high-Mn type Mn-Cu high damping alloy obtained in Example 1;
[0032] Figure 4 The damping strain amplitude curve diagram of the high-Mn type Mn-Cu high damping alloy obtained in Example 2;
[0033] Figure 5 The temperature-damping curve of the high-Mn type Mn-Cu high-damping alloy obtained in Example 2;
[0034] Figure 6 The temperature-modulus curve of the high-Mn type Mn-Cu high damping alloy obtained in Example 2;
[0035] Figure 7 The damping strain amplitude curve diagram of the high-Mn type Mn-Cu high damping alloy obtained in Example 3;
[0036] Figure 8 The temperature-damping curve of the high-Mn type Mn-Cu high-damping alloy obtained in Example 3;
[0037] Fig. 9 This is the temperature-modulus curve of the high Mn type Mn-Cu high damping alloy prepared in Example 3. DETAILED DESCRIPTION
[0038] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0039] Embodiment 1:
[0040] A high-Mn type Mn-Cu based high damping alloy comprises the following raw materials in percentage by mass: 22.5% Cu, 1.5% Al and 1% Sn, with the balance being Mn.
[0041] The preparation method of the above-mentioned high-Mn type Mn-Cu based high damping alloy comprises the following steps:
[0042] (1) Charging: Weigh the raw materials and dry them at 300°C for 24 hours, then mix and load them into the crucible in a ZG-25 vacuum induction furnace, place the casting ingot mold into the furnace, close the furnace door, and tighten the vent valve;
[0043] (2) Vacuuming: First, close the high vacuum valve, then open the low vacuum valve and mechanical pump in sequence, and finally open the pre-vacuum valve and turn on the power of the diffusion pump; when the vacuum degree reaches 500Pa, turn on the Roots pump to make the vacuum degree in the furnace reach 2-3Pa; use the diffusion pump to heat for 30 minutes to make the vacuum degree reach below 2Pa and close the low vacuum valve, open the high vacuum valve, so that the furnace reaches a high vacuum state;
[0044] (3) Melting: First, adjust the power of the vacuum induction furnace to 30 kW for melting until the raw materials are completely melted to obtain a liquid mixture, then adjust the power of the vacuum induction furnace to 0, fill with argon until the pressure reaches 0.06 MPa and then stop filling, finally adjust the power to 20 kW to continue melting until the raw materials are evenly mixed;
[0045] (4) Casting: Close the high vacuum valve and the Roots pump, and slowly cast the refined liquid mixture into the ingot mold. While casting, slowly reduce the power until the power is 0;
[0046] (5) Homogenization treatment: open the vent valve until the pressure inside the furnace reaches the external pressure, then open the furnace cover and use a crane to lift out the ingot mold containing the ingot. After the ingot is air-cooled to room temperature, keep it at 850°C for 24 hours, and then air-cool it to room temperature to complete homogenization annealing to obtain a cast alloy with uniform structure and composition.
[0047] (6) Forging: The cast alloy obtained in step (5) is forged at an initial forging temperature of 850° C. and a final forging temperature of 620° C. After air cooling to room temperature, a 400 mm×130 mm×15 mm plate-shaped forged alloy is obtained;
[0048] (7) Heat treatment: The plate-shaped forged alloy obtained in step (6) was kept at 880°C for 1 hour and then air-cooled to room temperature, and then kept at 360°C for 2 hours and then air-cooled to room temperature to obtain a high-Mn type Mn-Cu based high damping alloy Mn 75 Cu 22.5 Al 1.5 Sn1.
[0049] The sample obtained in Example 1 was cut into 30 mm × 10 mm × 1 mm samples to be tested, and then the damping performance, variable temperature damping performance, and variable temperature modulus curve were tested using a dynamic thermal mechanical analyzer (DMA Q800). The results are as follows: Figure 1-Figure 3 shown.
[0050] from Figure 1 It can be seen that Mn 75 Cu 22.5 Al 1.5 The damping property of Sn1 alloy is positively correlated with the strain amplitude. -6 ), the alloy's Tanδ≈0.02377; at a higher strain amplitude (800×10 -6 ), the alloy's Tanδ≈0.05131.
[0051] from Figure 2 It can be seen that Mn 75 Cu 22.5 Al 1.5 The relationship between the damping performance of Sn1 and temperature shows that as the temperature increases, the Tanδ of the alloy first decreases, and a wider temperature platform appears at room temperature. After the temperature rises to the As point, the damping performance of the alloy begins to decrease sharply.
[0052] from Figure 3 It can be seen that Mn 75 Cu 22.5 Al 1.5 The relationship between the storage modulus of Sn1 alloy and temperature shows that the modulus of the alloy reaches its lowest point as the temperature rises and falls. The temperatures corresponding to the lowest points are Ms (the lowest modulus during the cooling process) and As (the lowest modulus during the heating process). It can be seen that the As point of the alloy is 62.83℃, the Ms point is 126.89℃, and the phase transition points are above room temperature, so it can be used at higher temperatures.
[0053] Embodiment 2:
[0054] A high-Mn type Mn-Cu based high damping alloy comprises the following raw materials in percentage by mass: 24.5% Cu, 1.5% Al and 1% Sn, with the balance being Mn.
[0055] The preparation method of the above-mentioned high-Mn type Mn-Cu based high damping alloy comprises the following steps:
[0056] (1) Charging: Weigh the raw materials and dry them at 300°C for 24 hours, then mix and load them into the crucible in a ZG-25 vacuum induction furnace, place the casting ingot mold into the furnace, close the furnace door, and tighten the vent valve;
[0057] (2) Vacuuming: First, close the high vacuum valve, then open the low vacuum valve and mechanical pump in sequence, and finally open the pre-vacuum valve and turn on the power of the diffusion pump; when the vacuum degree reaches 500Pa, turn on the Roots pump to make the vacuum degree in the furnace reach 2-3Pa; use the diffusion pump to heat for 30 minutes to make the vacuum degree reach below 2Pa and close the low vacuum valve, open the high vacuum valve, so that the furnace reaches a high vacuum state;
[0058] (3) Melting: First, adjust the power of the vacuum induction furnace to 30 kW for melting until the raw materials are completely melted to obtain a liquid mixture, then adjust the power of the vacuum induction furnace to 0, fill with argon until the pressure reaches 0.06 MPa and then stop filling, finally adjust the power to 20 kW to continue melting until the raw materials are evenly mixed;
[0059] (4) Casting: Close the high vacuum valve and the Roots pump, and slowly cast the refined liquid mixture into the ingot mold. While casting, slowly reduce the power until the power is 0;
[0060] (5) Homogenization treatment: open the vent valve until the pressure inside the furnace reaches the external pressure, then open the furnace cover and use a crane to lift out the ingot mold containing the ingot. After the ingot is air-cooled to room temperature, keep it at 850°C for 24 hours, and then air-cool it to room temperature to complete homogenization annealing to obtain a cast alloy with uniform structure and composition.
[0061] (6) Forging: The cast alloy obtained in step (5) is forged at an initial forging temperature of 850° C. and a final forging temperature of 620° C. After air cooling to room temperature, a 400 mm×130 mm×15 mm plate-shaped forged alloy is obtained;
[0062] (7) Heat treatment: The plate-shaped forged alloy obtained in step (6) was kept at 880°C for 1 hour and then air-cooled to room temperature, and then kept at 360°C for 2 hours and then air-cooled to room temperature to obtain a high-Mn type Mn-Cu based high damping alloy Mn 73 Cu 24.5 Al 1.5 Sn1.
[0063] The sample obtained in Example 2 was cut into 30 mm × 10 mm × 1 mm samples to be tested, and then the damping performance, variable temperature damping performance, and variable temperature modulus curve were tested using a dynamic thermal mechanical analyzer (DMA Q800). The results are as follows: Figure 4-Figure 6 shown.
[0064] from Figure 4 It can be seen that Mn 73 Cu 24.5 Al 1.5 The damping property of Sn1 alloy is positively correlated with the strain amplitude. -6 ), the alloy's Tanδ≈0.02427; at a higher strain amplitude (800×10 -6 ), the alloy's Tanδ≈0.05778.
[0065] from Figure 5 It can be seen that Mn 73 Cu 24.5 Al 1.5 The relationship between the damping performance of Sn1 and temperature shows that as the temperature increases, the Tanδ of the alloy first decreases, and a wider temperature platform appears at room temperature. After the temperature rises to the As point, the damping performance of the alloy begins to decrease sharply.
[0066] from Figure 6 It can be seen that Mn 73 Cu 24.5 Al 1.5 The relationship between the storage modulus of Sn1 alloy and temperature shows that the modulus of the alloy reaches its lowest point as the temperature rises and falls. The temperatures corresponding to the lowest points are Ms (the lowest modulus during the cooling process) and As (the lowest modulus during the heating process). It can be seen that the As point of the alloy is 73.70℃, the Ms point is 136.69℃, and the phase transition points are above room temperature, so it can be used at higher temperatures.
[0067] Embodiment 3:
[0068] A high-Mn type Mn-Cu based high damping alloy comprises the following raw materials in percentage by mass: 26.5% Cu, 1.5% Al and 1% Sn, with the balance being Mn.
[0069] The preparation method of the above-mentioned high-Mn type Mn-Cu based high damping alloy comprises the following steps:
[0070] (1) Charging: Weigh the raw materials and dry them at 300°C for 24 hours, then mix and load them into the crucible in a ZG-25 vacuum induction furnace, place the casting ingot mold into the furnace, close the furnace door, and tighten the vent valve;
[0071] (2) Vacuuming: First, close the high vacuum valve, then open the low vacuum valve and mechanical pump in sequence, and finally open the pre-vacuum valve and turn on the power of the diffusion pump; when the vacuum degree reaches 500Pa, turn on the Roots pump to make the vacuum degree in the furnace reach 2-3Pa; use the diffusion pump to heat for 30 minutes to make the vacuum degree reach below 2Pa and close the low vacuum valve, open the high vacuum valve, so that the furnace reaches a high vacuum state;
[0072] (3) Melting: First, adjust the power of the vacuum induction furnace to 30 kW for melting until the raw materials are completely melted to obtain a liquid mixture, then adjust the power of the vacuum induction furnace to 0, fill with argon until the pressure reaches 0.06 MPa and then stop filling, finally adjust the power to 20 kW to continue melting until the raw materials are evenly mixed;
[0073] (4) Casting: Close the high vacuum valve and the Roots pump, and slowly cast the refined liquid mixture into the ingot mold. While casting, slowly reduce the power until the power is 0;
[0074] (5) Homogenization treatment: open the vent valve until the pressure inside the furnace reaches the external pressure, then open the furnace cover and use a crane to lift out the ingot mold containing the ingot. After the ingot is air-cooled to room temperature, keep it at 850°C for 24 hours, and then air-cool it to room temperature to complete homogenization annealing to obtain a cast alloy with uniform structure and composition.
[0075] (6) Forging: The cast alloy obtained in step (5) is forged at an initial forging temperature of 850° C. and a final forging temperature of 620° C. After air cooling to room temperature, a 400 mm×130 mm×15 mm plate-shaped forged alloy is obtained;
[0076] (7) Heat treatment: The plate-shaped forged alloy obtained in step (6) was kept at 880°C for 1 hour and then air-cooled to room temperature, and then kept at 360°C for 2 hours and then air-cooled to room temperature to obtain a high-Mn type Mn-Cu based high damping alloy Mn 71 Cu 26.5 Al 1.5 Sn1.
[0077] The sample obtained in Example 3 was cut into 30 mm × 10 mm × 1 mm samples to be tested, and then the damping performance, variable temperature damping performance, and variable temperature modulus curve were tested using a dynamic thermal mechanical analyzer (DMA Q800). The results are as follows: Figure 7-Figure 9 shown.
[0078] from Figure 7 It can be seen that Mn 71 Cu 26.5 Al 1.5 The damping property of Sn1 alloy is positively correlated with the strain amplitude. -6), the alloy's Tanδ≈0.02207; at a higher strain amplitude (800×10 -6 ), the alloy's Tanδ≈0.04665.
[0079] from Figure 8 It can be seen that Mn 71 Cu 26.5 Al 1.5 The relationship between the damping performance of Sn1 and temperature shows that as the temperature increases, the Tanδ of the alloy first decreases, and a wider temperature platform appears at room temperature. After the temperature rises to the As point, the damping performance of the alloy begins to decrease sharply.
[0080] from Fig. 9 It can be seen that Mn 71 Cu 26.5 Al 1.5 The relationship between the storage modulus of Sn1 alloy and temperature shows that the modulus of the alloy reaches its lowest point as the temperature rises and falls. The temperatures corresponding to the lowest points are Ms (the lowest modulus during the cooling process) and As (the lowest modulus during the heating process). It can be seen that the As point of the alloy is 70.86℃, the Ms point is 134.15℃, and the phase transition points are above room temperature, so it can be used at higher temperatures.
[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A high Mn type Mn-Cu based high damping alloy, It is characterized in that The invention comprises the following raw materials in percentage by mass: Cu 22.5-26.5%, Al 1-2% and Sn 0.8-1.2%, and the balance is Mn.
2. The high Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that The raw materials include the following mass percentages: Cu 22.5%, Al 1.5% and Sn 1%, and the balance is Mn; or Cu 24.5%, Al 1.5% and Sn 1%, and the balance is Mn; or Cu 26.5%, Al 1.5% and Sn 1%, and the balance is Mn.
3. A method for preparing the high Mn type Mn-Cu based high damping alloy according to claim 1 or 2, It is characterized in that The following steps are involved: The raw materials are first mixed and smelted, and then rare gas is added to continue smelting, and then cast to obtain an alloy ingot, and finally the obtained alloy ingot is annealed, forged and heat treated to obtain the alloy.
4. The method for preparing the high-Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that The smelting power is 28-32kW, and the smelting is carried out until the raw materials are completely melted.
5. The method for preparing the high Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that Fill with rare gas until the pressure reaches 0.05-0.07Mpa, continue smelting at a power of 18-22kW, and continue smelting until the raw materials are evenly mixed.
6. The method for preparing the high Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that Annealing conditions are: keep at 800-900℃ for 20-30h and then air cool to room temperature.
7. The method for preparing the high-Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that The starting forging temperature of forging is 800-900℃, and the ending forging temperature is 600-650℃.
8. The method for preparing the high-Mn type Mn-Cu based high damping alloy according to claim 1, It is characterized in that The heat treatment conditions are: first keep at 850-900°C for 0.5-2h and then air cool to room temperature, then keep at 350-380°C for 1-3h and then air cool to room temperature to complete the heat treatment.
9. Use of the high-Mn type Mn-Cu based high damping alloy according to claim 1 or 2 in reducing vibration and noise in industry.