Method for improving uniformity of nitriding layer of G13Cr4Mo4Ni4V steel ferrule

The method addresses low efficiency and shallow nitriding issues by optimizing pretreatment and nitriding parameters, achieving uniform nitriding layer depth and improved hardness and stress uniformity in G13Cr4Mo4Ni4V steel ferrules.

CN119082660APending Publication Date: 2024-12-06AVIC HARBIN BEARING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191176.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional ion nitriding methods for G13Cr4Mo4Ni4V steel ferrules suffer from low efficiency, shallow nitriding layer, and poor uniformity, leading to inconsistencies in hardness and stress indicators, affecting dimensional stability and fatigue performance.

Method used

A method involving workpiece pretreatment, optimized clamping in a vacuum furnace, and controlled nitriding process parameters, including temperature and support method, to enhance nitriding layer uniformity and depth.

Benefits of technology

Improves the uniformity and depth of the nitriding layer, enhancing hardness and stress uniformity, ensuring dimensional stability and reliability of the nitrided bearing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082660A_ABST
    Figure CN119082660A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving the uniformity of a nitriding layer of a G13Cr4Mo4Ni4V steel ferrule, in particular to a method for improving the uniformity of a nitriding layer of a G13Cr4Mo4Ni4V steel ferrule. The invention aims to solve the problems of low conventional nitriding efficiency and shallow nitriding layer. The method comprises the steps that 1, workpiece pretreatment is conducted, specifically, rough turning, carburizing treatment, annealing, fine turning, quenching and tempering, demagnetization, rough grinding machining, stabilizing treatment and fine grinding machining are conducted on the G13Cr4Mo4Ni4V steel bearing ring in sequence, and the finely-ground G13Cr4Mo4Ni4V steel bearing ring is obtained; secondly, the G13Cr4Mo4Ni4V steel bearing ring obtained after fine grinding is subjected to tool clamping and evenly placed in a vacuum nitriding furnace in a supporting mode, and a part to be nitrided is obtained; and thirdly, nitriding treatment is conducted on the part to be nitrided. The method is used for improving the uniformity of the nitriding layer of the G13Cr4Mo4Ni4V steel ferrule.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for improving the uniformity of a nitriding layer of a G13Cr4Mo4Ni4V steel ferrule. Background Art

[0002] Ion nitriding is an effective means to improve the surface hardness, fatigue strength, wear resistance and corrosion resistance of steel, and is widely used in the production and manufacturing of tooling, molds, and weapon equipment parts. However, as a high-alloy steel, G13Cr4Mo4Ni4V has the problems of low nitriding efficiency and shallow nitriding layer, and is currently mostly in the sample level research. G13Cr4Mo4Ni4V high-temperature carburized bearings are a common material for bearing steel rings, and the uniformity of the nitriding layer of the steel ring and the effective nitriding layer depth of the final product need to be comprehensively considered.

[0003] At the same time, the nitriding treatment of the rings also has problems such as glow and deformation, which leads to insufficient effective nitriding layer depth of the final product and cannot effectively improve the hardness and stress indicators. At the same time, poor uniformity of the nitriding layer will cause differences in hardness and stress indicators, affecting the dimensional stability and fatigue performance of the rings. In summary, improving the uniformity of the nitriding layer of the final product of the bearing ring is the core of the application of this technology. Summary of the invention

[0004] The purpose of the present invention is to solve the problems of low efficiency and shallow nitriding layer of conventional nitriding and to provide a method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule.

[0005] The method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule of the present invention is specifically carried out according to the following steps:

[0006] 1. Workpiece pretreatment: The G13Cr4Mo4Ni4V steel bearing ring is subjected to rough turning, carburizing, annealing, fine turning, quenching and tempering, demagnetization, rough grinding, stabilization and fine grinding in sequence to obtain the finely ground G13Cr4Mo4Ni4V steel bearing ring;

[0007] 2. The finely ground G13Cr4Mo4Ni4V steel bearing ring is clamped and evenly placed in the vacuum nitriding furnace in a supporting manner to obtain the part to be nitrided;

[0008] 3. Carry out nitriding treatment on the parts to be nitrided.

[0009] Beneficial effects of the present invention:

[0010] By rationally designing the nitriding tooling, optimizing the loading method and the position of the temperature control couple, the uniformity of the nitriding layer of the bearing after nitriding is improved; by eliminating the residual stress before nitriding and controlling the grinding amount after nitriding, the effective nitriding layer depth is increased. In this way, the uniformity of the nitriding layer of the finished nitrided bearing is controlled within 0.05mm, and the hardness and stress uniformity of the bearing are improved simultaneously, ensuring the dimensional stability and reliability of the nitrided bearing. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a schematic diagram of three-point support; 1 represents the bearing ring, and 2 represents the three-point support;

[0012] Figure 2 Schematic diagram of the arrangement of temperature control couples; 3 represents the temperature control couple, and 4 represents the part to be nitrided. DETAILED DESCRIPTION

[0013] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes. The following specific implementation modes are described in conjunction with the accompanying drawings.

[0014] Specific implementation method 1: This implementation method is a method for improving the uniformity of the nitriding layer of the G13Cr4Mo4Ni4V steel ferrule, which is specifically carried out according to the following steps:

[0015] 1. Workpiece pretreatment: The G13Cr4Mo4Ni4V steel bearing ring is subjected to rough turning, carburizing, annealing, fine turning, quenching and tempering, demagnetization, rough grinding, stabilization and fine grinding in sequence to obtain the finely ground G13Cr4Mo4Ni4V steel bearing ring;

[0016] 2. The finely ground G13Cr4Mo4Ni4V steel bearing ring is clamped and evenly placed in the vacuum nitriding furnace in a supporting manner to obtain the part to be nitrided;

[0017] 3. Carry out nitriding treatment on the parts to be nitrided.

[0018] In this embodiment, the parts need to be fully cleaned before nitriding treatment to ensure that there are no defects such as rust and pitting on the surface of the parts, and no impurities such as oil stains. At the same time, in order to fully release the residual stress generated by forging and grinding before nitriding, and to promote the full transformation of residual austenite, stabilization treatment is performed before fine grinding.

[0019] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that the specific process parameters of the rough turning in step 1 are that the turning amount per turn does not exceed 1.5 mm, and the line speed is controlled at 150-170 m / min; the specific process parameters of the fine turning are that the turning amount per turn does not exceed 0.3 mm, and the line speed is controlled at 90-110 m / min. The rest is the same as the specific embodiment 1.

[0020] This embodiment controls the turning amount and reduces the uneven internal stress caused by machining.

[0021] Specific embodiment 3: This embodiment is different from specific embodiment 1 in that the specific process parameters of the carburizing treatment in step 1 are that the carburizing temperature is controlled at 930-980°C, the carburizing time is controlled at 30-40h, and the cooling pressure does not exceed 2bar. Others are the same as specific embodiment 1.

[0022] Specific implementation method 4: This implementation method is different from specific implementation method 1 in that the specific process parameters of the annealing in step 1 are annealing at 680-720° C. for not less than 8 hours. The rest is the same as specific implementation method 1.

[0023] Specific embodiment 5: This embodiment is different from specific embodiment 1 in that: the specific process parameters of quenching and tempering in step 1 are that the quenching temperature is controlled at 1070-1100°C, the quenching pressure is 2-4 bar, the tempering temperature is controlled at 530-550°C, and the tempering time is controlled at 2-4 hours. The rest is the same as specific embodiment 1.

[0024] Specific implementation method 6: This implementation method is different from the specific implementation method 1 in that the residual magnetism content after demagnetization in step 1 is ≤ 1H / m. Other aspects are the same as those of the specific implementation method 1.

[0025] Specific implementation method 7: This implementation method is different from the specific implementation method 1 in that the specific process parameters of the rough grinding process in step 1 are that the single grinding depth is controlled between 0.002 and 0.005 mm, the workpiece linear speed is controlled between 10 and 15 m / min, the worktable speed is 80 to 120 mm / min, and the grinding wheel speed is not higher than 80,000 r / min. Others are the same as the specific implementation method 1.

[0026] Specific embodiment eight: This embodiment differs from specific embodiment one in that: the stabilization treatment in step one is to keep the temperature at 300-450°C for 3-5 hours to complete the high temperature treatment; then transfer to a cold treatment furnace and keep the temperature at -75°C for 3-4 hours to complete the low temperature treatment; repeat the high and low temperature treatment 3-5 times to complete the nitriding stabilization treatment. The rest is the same as specific embodiment one.

[0027] This implementation ensures that the initial residual stress is fully released, reduces the deformation caused by stress release during the nitriding process, can reduce the deformation of the bearing after nitriding, and improves the overall dimensional stability of the bearing.

[0028] Specific implementation method 9: This implementation method is different from specific implementation method 1 in that: in step 2, the distance between the outer walls of each tooling is not less than 20 mm, and the support method is three-point support. Other aspects are the same as specific implementation method 1.

[0029] In the present embodiment, the bearing ring nitriding process adopts a support method to carry out nitriding, so as to prevent the contact surface between the ring and the fixture from being without glow, causing temperature difference and thus poor uniformity of the nitriding layer. The support adopts three-point support to reduce the influence of the support on the bending of the ring.

[0030] The tooling design in this embodiment needs to ensure that the tooling and the parts are fully fitted, but it does not affect the overall heating and cooling of the bearing parts, and does not affect the nitriding efficiency of the bearing parts. The tooling should minimize irregular structures to ensure that the parts are heated evenly; after the parts and tooling are combined, they must be evenly placed in the furnace, and the distance between the outer walls of each tooling should not be less than 20mm to avoid mutual glow affecting the heating uniformity.

[0031] Specific embodiment ten: This embodiment differs from specific embodiment nine in that: the process parameters of the nitriding treatment in step three are: the ion nitriding temperature is selected from 480 to 515°C, the nitriding time is selected from 50 to 70 hours, the nitriding voltage is 500 to 520V, the surface activation voltage is 590 to 630V, and the gas pressure is 1 to 4 mbar; a temperature control couple and a temperature measuring couple are set during the nitriding process; the temperature control couple and the temperature measuring couple are both supported by three points. The rest is the same as specific embodiment nine.

[0032] This implementation can ensure that the thermocouple can accurately and timely feedback the temperature of the nitrided part.

[0033] The temperature measuring couple in this embodiment is generally randomly tied to a certain workpiece.

[0034] After the bearing ring of this embodiment is nitrided, the surface hardness is significantly improved. Therefore, the subsequent grinding should appropriately control the amount of single-pass grinding to ensure that the amount of grinding removal per pass is no more than 0.02 mm, thereby reducing the subsequent grinding deformation of the ring.

[0035] The beneficial effects of the present invention are verified by the following examples:

[0036] Embodiment: A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule is specifically carried out according to the following steps:

[0037] 1. Workpiece pretreatment: The G13Cr4Mo4Ni4V steel bearing ring is subjected to rough turning, carburizing, annealing, fine turning, quenching and tempering, demagnetization, rough grinding, stabilization and fine grinding in sequence to obtain the finely ground G13Cr4Mo4Ni4V steel bearing ring; the specific process parameters of the rough turning are that the turning amount does not exceed 1.5mm per time, and the line speed is controlled at 150-170m / min; the specific process parameters of the fine turning are that the turning amount does not exceed 0.3mm per time, and the line speed is controlled at 90-110m / min; the specific process parameters of the carburizing treatment are that the carburizing temperature is controlled at 930-980℃, the carburizing time is controlled at 30-40h, and the cooling pressure does not exceed 2bar; the specific process parameters of the annealing are annealing at 680-720℃ for not less than 8h; The specific process parameters of quenching and tempering are as follows: the quenching temperature is controlled at 1070-1100°C, the quenching pressure is 2-4 bar; the tempering temperature is controlled at 530-550°C, and the tempering time is controlled at 2-4 hours; the residual magnetism content after demagnetization is ≤1H / m; the specific process parameters of the rough grinding process are as follows: the single grinding depth is controlled between 0.002-0.005mm, the workpiece linear speed is controlled at 10-15m / min, the worktable speed is 80-120mm / min, and the grinding wheel speed is not higher than 80000r / min; the stabilization treatment is carried out at a temperature of 300-450°C for 3-5 hours to complete the high-temperature treatment; then the product is transferred to a cold treatment furnace and kept at a temperature of -75°C for 3-4 hours to complete the low-temperature treatment; the high and low temperature treatment is repeated 3-5 times to complete the nitriding stabilization treatment;

[0038] 2. The finely ground G13Cr4Mo4Ni4V steel bearing ring is clamped by a tool and evenly placed in a vacuum nitriding furnace by a support method to obtain a part to be nitrided; the distance between the outer walls of each tool is not less than 20 mm, and the support method is a three-point support;

[0039] 3. Perform nitriding treatment on the parts to be nitrided; the process parameters of the nitriding treatment are as follows: the ion nitriding temperature is selected at 480-515°C, the nitriding time is selected at 50-70h, the nitriding voltage is 500-520V, the surface activation voltage is 590-630V, and the gas pressure is 1-4mbar; a temperature control couple and a temperature measuring couple are set during the nitriding process; the temperature control couple and the temperature measuring couple are both supported by three points.

[0040] The surface hardness of G13Cr4Mo4Ni4V high temperature carburized bearing steel reaches 900HV after ion nitriding treatment 0.3Compared with conventional carburizing treatment, 730HV is further improved, the surface residual compressive stress reaches above -500MPa, the maximum residual compressive stress reaches above -700MPa, and the depth of the compressive stress layer reaches above -350μm. Compared with conventional carburizing hardening treatment, the hardness of the bearing working surface is further improved, and the compressive stress level is significantly improved.

Claims

1. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule. Features The method for improving the uniformity of the nitriding layer of the G13Cr4Mo4Ni4V steel ferrule is specifically carried out in the following steps:

1. Workpiece pretreatment: The G13Cr4Mo4Ni4V steel bearing ring is subjected to rough turning, carburizing, annealing, fine turning, quenching and tempering, demagnetization, rough grinding, stabilization and fine grinding in sequence to obtain the finely ground G13Cr4Mo4Ni4V steel bearing ring; 2. The finely ground G13Cr4Mo4Ni4V steel bearing ring is clamped and evenly placed in the vacuum nitriding furnace in a supporting manner to obtain the part to be nitrided; 3. Carry out nitriding treatment on the parts to be nitrided.

2. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The specific process parameters of the rough turning in step one are that the single turning amount does not exceed 1.5 mm, and the line speed is controlled at 150-170 m / min; the specific process parameters of the fine turning are that the single turning amount does not exceed 0.3 mm, and the line speed is controlled at 90-110 m / min.

3. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The specific process parameters of the carburizing treatment in step 1 are that the carburizing temperature is controlled at 930-980° C., the carburizing time is controlled at 30-40 hours, and the cooling pressure does not exceed 2 bar.

4. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The specific process parameters of the annealing in step 1 are annealing at 680-720° C. for not less than 8 hours.

5. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The specific process parameters of the quenching and tempering in step 1 are: the quenching temperature is controlled at 1070-1100°C, the quenching pressure is controlled at 2-4 bar; the tempering temperature is controlled at 530-550°C, and the tempering time is controlled at 2-4 hours.

6. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The residual magnetism content after demagnetization in step 1 is ≤1H / m.

7. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The specific process parameters of the rough grinding process in step 1 are as follows: the single grinding depth is controlled between 0.002 and 0.005 mm, the workpiece linear speed is controlled between 10 and 15 m / min, the worktable speed is 80 to 120 mm / min, and the grinding wheel speed is not higher than 80,000 r / min.

8. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The stabilization treatment in step 1 is to keep the temperature at 300-450°C for 3-5 hours to complete the high temperature treatment; then transfer to a cold treatment furnace and keep the temperature at -75°C for 3-4 hours to complete the low temperature treatment; repeat the high and low temperature treatment 3-5 times to complete the nitriding stabilization treatment.

9. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features In step 2, the distance between the outer walls of each tooling is not less than 20 mm, and the support method is three-point support.

10. A method for improving the uniformity of the nitriding layer of a G13Cr4Mo4Ni4V steel ferrule according to claim 1, Features The process parameters of the nitriding treatment in step three are as follows: the ion nitriding temperature is selected at 480-515°C, the nitriding time is selected at 50-70h, the nitriding voltage is 500-520V, the surface activation voltage is 590-630V, and the gas pressure is 1-4mbar; a temperature control couple and a temperature measuring couple are set during the nitriding process; the temperature control couple and the temperature measuring couple are both supported by three points.