Large-area WC superconducting film prepared by magnetron sputtering

Magnetron sputtering technology allows for efficient production of large-area WC superconducting films with uniform thickness and superconductivity, addressing industrial production limitations and enabling high-performance superconducting devices.

CN119082667AActive Publication Date: 2024-12-06NANJING UNIV OF SCI & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411191760.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Existing methods for preparing WC films, such as chemical vapor deposition, are complex and limit industrial production, while other methods like solid, gas, and liquid phase methods have inefficiencies or complications, making them unsuitable for large-scale production of high-quality WC superconducting materials.

Method used

A large-area WC superconducting film is prepared using magnetron sputtering technology on a substrate, with an optional Al protective layer to prevent oxidation, and controlled sputtering temperatures to achieve uniform thickness and superconductivity.

Benefits of technology

The method enables efficient, large-area WC film production with uniform thickness and superconducting properties, suitable for industrial mass production, and can be used in superconducting devices with improved sensitivity and reduced power consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082667A_ABST
    Figure CN119082667A_ABST
Patent Text Reader

Abstract

The invention discloses a large-area WC superconducting film prepared by magnetron sputtering, and belongs to the technical field of superconducting materials. The method comprises the following steps: preparing a WC film with the thickness of 7 nm on a cleaned sapphire substrate by using a magnetron sputtering technology, wherein the sputtering temperature is room temperature or 500 DEG C; the large-area WC superconducting thin film can be produced through the magnetron sputtering technology, the WC superconducting thin film is uniform in thickness, low in technological operation difficulty, simple in technological process, high in efficiency and high in repetition rate, and the WC superconducting thin film can serve as a superconducting material and is very suitable for manufacturing wafer-level superconducting thin film electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of superconducting thin film materials, and in particular relates to a large-area WC film with superconductivity prepared by magnetron sputtering technology. Background Art

[0002] Superconducting materials are new materials with three basic properties: zero resistance, complete anti-magnetism, and macroscopic quantum effects. Based on the zero resistance and complete anti-magnetism of superconducting materials, applying large currents in superconducting materials can realize technologies such as large current transport, strong magnetic fields, and magnetic levitation; based on the quantum tunneling effect, superconductivity can be applied to quantum computing and weak magnetic field detection. Therefore, superconducting materials are widely used in many fields such as power transmission, medical equipment, electronic communications, and national defense and military. Superconducting electronic devices are a type of electronic devices developed based on the principle of superconductivity. Compared with ordinary electronic devices, they have faster response rates, lower energy consumption, and higher computing accuracy. Superconducting electronic devices have broad application prospects in superconducting quantum computing, superconducting electric vehicles, and power transmission.

[0003] At present, the preparation forms of WC materials mainly include WC powder, WC film, etc. The three mainstream WC powder material preparation methods are solid phase method, gas phase method and liquid phase method. Among them, the solid phase method has simple process operation and good uniformity of powder product particle size, but its production efficiency is low and impurities are easily introduced in the process. The gas phase method can be used to prepare powder products with finer particle size, but the reaction temperature required for its production process is relatively high. The liquid phase method can also be used to prepare WC powder materials with finer particle size, and the requirements for the reaction temperature environment are relatively low, but its preparation process is complicated and the feasibility of mass production application is low. WC films are mainly obtained by chemical vapor deposition (CVD) and physical vapor deposition (PVD). However, the complex process of chemical vapor deposition limits the industrial production of WC films from the laboratory. Summary of the invention

[0004] The purpose of the present invention is to provide a large-area WC superconducting film, which can be grown on the entire substrate by magnetron sputtering equipment and is particularly suitable for industrial mass growth.

[0005] The technical solution to achieve the purpose of the present invention is:

[0006] In a first aspect, the present invention provides a large-area WC superconducting film, which is prepared on a substrate by magnetron sputtering technology.

[0007] Preferably, in order to prevent the WC superconducting film from being oxidized, an Al protective layer is prepared on the WC superconducting film by magnetron sputtering technology.

[0008] Preferably, the substrate is a rigid substrate commonly used in the art, such as (0001) crystal plane single crystal sapphire.

[0009] Preferably, the WC superconducting film has a thickness of 7 nm;

[0010] In a second aspect, the present invention provides a method for preparing a large-area WC superconducting film as described in the first aspect, comprising the following steps: using a WC target as a target material, performing vacuum magnetron sputtering on a clean substrate, and the sputtering temperature is room temperature or 500°C.

[0011] Preferably, the cleaned substrate refers to the substrate being ultrasonically cleaned for 10 minutes using acetone and anhydrous ethanol in sequence, and then blown dry using a nitrogen gun.

[0012] Preferably, the purity of the WC target is 99.9%.

[0013] Preferably, the protective gas is argon with a purity of 99.995%, and the sputtering gas pressure is 0.6Pa.

[0014] In a third aspect, the present invention provides a use of the large-area WC superconducting film described in the first aspect as a superconducting material.

[0015] Preferably, the WC superconducting film prepared when the sputtering temperature is room temperature has a resistance of 0 at a temperature of 4.4K, and has a superconducting phenomenon.

[0016] Preferably, the WC superconducting film prepared at a sputtering temperature of 500° C. has a resistance of 0 at a temperature of 3.93K, and exhibits a superconducting phenomenon.

[0017] In a fourth aspect, the present invention provides a superconducting sensor / detector, which comprises the large-area WC superconducting film described in the first aspect.

[0018] In a fifth aspect, the present invention provides a microwave resonant cavity comprising the large-area WC superconducting film described in the first aspect.

[0019] In a sixth aspect, the present invention provides a superconducting digital circuit, which comprises the large-area WC superconducting film described in the first aspect.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention utilizes magnetron sputtering technology, and by changing the temperature of the sputtering chamber, controls the growth temperature of the WC film, and produces a large area of ​​continuous film with uniform thickness. The process flow is simple, efficient, and repetitive, and it is a production method suitable for industrial level. The WC film prepared by this method has a superconducting phenomenon at a certain temperature, and the WC superconducting device prepared by the subsequent micro-nano processing technology has broad application prospects in the field of superconducting electronics research: first, the steep superconducting transition of the superconducting material can be used to achieve the high sensitivity of the superconducting sensor / detector, so that it has broad application prospects in the fields of superconducting quantum interference devices, superconducting nanowire single photon detectors, high-temperature superconducting terahertz technology, etc.; second, when microwaves pass through the surface of the superconducting material, its microwave surface resistance is very small, so the microwave resonant cavity prepared by the superconducting material has extremely small microwave loss, and the prepared superconducting filter has very small insertion loss, and the performance is significantly improved compared with the conventional filter; third, the superconducting digital circuit has lower power consumption, smaller size and lower signal loss than the semiconductor digital circuit.

[0022] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0024] Figure 1 This is the Raman spectrum of the WC film prepared in Example 1 of the present invention.

[0025] Figure 2 This is the Raman spectrum of the WC film prepared in Example 2 of the present invention.

[0026] Figure 3 This is a low-resolution transmission electron microscope image of the WC film prepared in Example 3 of the present invention.

[0027] Figure 4 This is a low-resolution transmission electron microscope image of the WC film prepared in Example 4 of the present invention.

[0028] Figure 5 This is the resistance-temperature (RT) curve of WC prepared in Example 5 of the present invention.

[0029] Figure 6 This is the resistance-temperature (RT) curve of WC prepared in Example 6 of the present invention. DETAILED DESCRIPTION

[0030] The present application is further described below in conjunction with specific embodiments.

[0031] It should be noted that the terms such as "upper", "lower", "left", "right", "middle", etc. cited in this specification are only for the convenience of description and are not used to limit the scope of implementation. Changes or adjustments to their relative relationships should be regarded as the scope of implementation of this application without substantially changing the technical content.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.

[0033] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0034] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.

[0035] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.

[0036] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values ​​or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values ​​and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.

[0037] The magnetron sputtering technology provided by the present invention for preparing large-area WC thin films is an important physical vapor deposition method with a low deposition temperature and a high deposition rate, which can simplify the preparation process, reduce production costs, and be better suitable for industrial mass production. The room temperature WC film and the 500°C WC film prepared by the magnetron sputtering technology were prepared into six-electrode Hall devices using ultraviolet lithography and ion etching technology. When the longitudinal resistance of the WC Hall device at different temperatures was tested by the magnetoelectric transport system, it was accidentally discovered that both the room temperature WC film and the 500°C WC film showed superconductivity, which can be used for the subsequent preparation of WC superconducting devices and have higher industrial value compared with WC powder.

[0038] Embodiment 1:

[0039] In this embodiment, the thickness of the WC film is 7 nm.

[0040] The specific steps are as follows:

[0041] Step (1): Cut a 2-inch sapphire wafer into 1×1 cm sizes.

[0042] Step (2): The cut sapphire substrate is cleaned for 10 minutes in acetone with an industrial purity of more than 99.95% or anhydrous ethanol with a purity of more than 99.97% using an ultrasonic machine, and then blown dry with a nitrogen gun.

[0043] Step (3): Install a WC target material with a purity of 99.9% and a diameter of 50.8 mm on the DC target position of magnetron sputtering; and fix the cleaned sapphire substrate on the sample holder.

[0044] Step (4): Use mechanical pumps and molecular pumps to pump the vacuum degree of the vacuum sputtering chamber to a value better than 5×10 -5 Pa.

[0045] Step (5): Maintain the temperature of the sputtering chamber at room temperature, introduce 99.995% argon as the working gas, adjust the sputtering gas pressure to 0.6 Pa, adjust the DC power supply power to 20 W, and adjust the spin rate of the sample holder to 20 rpm, and the sputtering rate is 0.067 nm / s.

[0046] Step (6): Open the shutter to start sputtering for 104.5 seconds, then close the shutter to obtain a WC film with a thickness of 7 nm.

[0047] The Raman spectrum of the WC superconducting film prepared in Example 1 is as follows: Figure 1 As shown, Figure 1 It can be seen that the horizontal axis is 750cm -1 、800cm -1 、1350cm -1 、1580cm-1 The Raman characteristic peak of WC that appears nearby is consistent with that reported in the literature. In addition, the characteristic peaks of the samples were tested at multiple locations, and they remained consistent, proving the uniformity of the film.

[0048] Example 2

[0049] The other processes are the same as those in Example 1, except that the temperature of the sputtering chamber in step (5) is adjusted to 500°C.

[0050] The Raman spectrum of the WC superconducting film prepared in this example is as follows: Figure 2 As shown, Figure 2 It can be seen that the horizontal axis is 750cm -1 、800cm -1 、1350cm -1 、1580cm -1 The Raman characteristic peak of WC that appears nearby is consistent with that reported in the literature. In addition, the characteristic peaks of the samples were tested at multiple locations, and they remained consistent, proving the uniformity of the film.

[0051] Example 3

[0052] All the processes of the WC film in this embodiment are the same as those in Embodiment 1, except that the morphology of the WC film is characterized by a transmission electron microscope.

[0053] The low-resolution transmission electron microscopy image of the WC film prepared in this example is as follows: Figure 3 As shown, a WC film with very good continuity and flatness was prepared.

[0054] Example 4

[0055] All the processes of the WC film in this embodiment are the same as those in Embodiment 2, except that the morphology of the WC film is characterized by a transmission electron microscope.

[0056] The low-resolution transmission electron microscopy image of the WC film prepared in this example is as follows: Figure 4 As shown, a WC film with very good continuity and flatness was prepared.

[0057] Example 5

[0058] The WC film prepared in Example 1 was prepared into a six-electrode Hall device using ultraviolet lithography and ion etching technology, and a 0.1 mA direct current was applied to test the longitudinal resistance of the WC Hall device at different temperatures.

[0059] The temperature-resistance (RT) curve of the WC Hall device prepared in this embodiment is as follows: Figure 5 As shown. Figure 5 It can be seen that the resistance of WC drops to 0 at a temperature of 4.4K, indicating the occurrence of superconductivity.

[0060] Example 6

[0061] The WC film prepared in Example 2 was prepared into a six-electrode Hall device using ultraviolet lithography and ion etching technology, and a 0.1 mA direct current was applied to test the longitudinal resistance of the WC Hall device at different temperatures.

[0062] The temperature-resistance (RT) curve of the WC Hall device prepared in this embodiment is as follows: Figure 6 As shown. Figure 6 It can be seen that the resistance of WC drops to 0 at a temperature of 3.93K, indicating the occurrence of superconductivity.

[0063] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the present invention is defined by the attached claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any figure mark in the claims should not be regarded as limiting the claims involved. At the same time, for those of ordinary skill in the art, without departing from the precursor of the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A large-area WC superconducting film, characterized in that: It is characterized in that The WC superconducting film is prepared on a substrate by magnetron sputtering technology.

2. The WC superconducting film according to claim 1, characterized in that: An Al protective layer is prepared on the WC superconducting film by magnetron sputtering technology.

3. The WC superconducting film according to claim 1, characterized in that: The WC superconducting film has a thickness of 7 nm.

4. A method for preparing a large-area WC superconducting film as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: using a WC target as a target, performing vacuum magnetron sputtering on a clean substrate, and the sputtering temperature is room temperature or 500 ºC.

5. Use of the large-area WC superconducting film as claimed in any one of claims 1 to 3 as a superconducting material.

6. The use according to claim 5, characterized in that The WC superconducting film prepared when the sputtering temperature is room temperature has a resistance of 0 at a temperature of 4.4 K, indicating superconductivity.

7. The use according to claim 5, characterized in that The WC superconducting film prepared at a sputtering temperature of 500 ºC has a resistance of 0 at a temperature of 3.93 K, indicating superconductivity.

8. A superconducting sensor / detector, characterized in that: It comprises the large-area WC superconducting film as claimed in any one of claims 1-3.

9. A microwave resonant cavity, characterized in that: It comprises the large-area WC superconducting film as claimed in any one of claims 1-3.

10. A superconducting digital circuit, characterized in that: It comprises the large-area WC superconducting film as claimed in any one of claims 1-3.

Citation Information

Patent Citations

  • Method for preparing NbTi film by utilizing magnetron sputtering method

    CN101914753A

  • Transparent conductive WC thin film and room temperature growth method thereof

    CN108182987A

  • Production method of high-temp. superconducting film

    CN1254191A

  • Device system generating extremely high compressive stresses and high (synthesis) temperatures, for the direct encapsulation of physicochemical products

    DE102022003959A1

  • Formation of deposited film

    JP1987142780A