Preparation method of low-surface-energy corrosion-resistant super-hydrophobic coating on zinc alloy surface

The formation of CoMIx coating on the surface of zinc alloy by surface replacement and in-situ growth methods solves the problem of corrosion on the surface of zinc alloy, and realizes the improvement of superhydrophobic performance and self-cleaning function, simplifies the process flow, reduces costs, and is suitable for industrialization Production.

CN119082730APending Publication Date: 2024-12-06CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411195488.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, zinc alloy surface is prone to corrosion, and the preparation of superhydrophobic coatings is complicated, energy consumption is high, and equipment requirements are high, making it difficult to achieve industrial production.

Method used

Using surface replacement and in-situ growth methods, a CoMIx coating with a layered sheet structure was formed on the surface of the zinc alloy, and a coating with superhydrophobic properties was prepared by a combination of pretreatment, replacement solution, growth solution and low surface energy solution.

Benefits of technology

It has achieved the improvement of low surface energy, corrosion resistance and self-cleaning performance of zinc alloy surfaces. It has simple process, low cost, wide application range, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082730A_ABST
    Figure CN119082730A_ABST
Patent Text Reader

Abstract

The invention relates to the field of metal material surface modification, and provides a preparation method of a zinc alloy surface low-surface-energy corrosion-resistant super-hydrophobic coating, which comprises the following steps: (1) zinc alloy surface pretreatment; and (2) preparing the coating: vertically placing the treated zinc alloy in a replacement solution, standing for a period of time, washing, then vertically placing in a growth solution, standing for a period of time, taking out, washing, then vertically placing in a constant-temperature low-surface-energy solution, standing for a period of time, taking out, washing, and drying, so as to obtain the low-surface-energy CoMIx coating on the surface of the zinc alloy. According to the method, the CoMIx coating with the lamellar structure is prepared on the surface of the zinc alloy through the surface replacement and in-situ growth method, the zinc alloy surface is subjected to stearic acid low-energy modification to obtain the super-hydrophobic function, the method is simple in process, the reaction process is easy to control, the production efficiency is high, the cost is low, the corrosion resistance and the self-cleaning performance of the zinc alloy are improved, and the application prospect is wide. The industrial production is favorably realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of surface modification of metal materials, and in particular to a method for preparing a low surface energy, corrosion-resistant and super-hydrophobic coating on a zinc alloy surface. Background Art

[0002] Zinc alloy is often used to manufacture outdoor lighting accessories due to its excellent corrosion resistance and good mechanical properties. However, when these lamps are exposed to marine climates containing salt and moisture for a long time, the zinc alloy surface may corrode and form a layer of white frost-like corrosion products, which not only affects the appearance of the lamps, but also may weaken their structural strength, leading to premature failure of the lamps.

[0003] Superhydrophobicity is manifested as a high contact angle (greater than 150°) and a low rolling angle (less than 10°). Superhydrophobic surfaces usually have a rough structure at the micro-nano level, showing excellent properties such as self-cleaning, drag reduction, and low adhesion. When liquid drops on a superhydrophobic surface, due to the combined effect of the rough micro-nano structure and low surface energy, an "air cushion" will be formed between the liquid and the surface, effectively preventing the direct contact between the corrosive medium and the substrate, thereby providing a certain degree of protection for the substrate. Therefore, introducing superhydrophobic surface technology into the field of metal surface modification can not only enhance the corrosion resistance of the substrate, but also give it a variety of functional properties such as self-cleaning.

[0004] At present, researchers have successfully prepared super-hydrophobic coatings with special functions such as corrosion resistance, self-cleaning, oil-water separation, and anti-icing through various methods such as hydrothermal method, plasma spray method, and electrochemical deposition method. However, the hydrothermal method requires expensive high-temperature and high-pressure equipment, and there are safety risks in operation, high energy consumption, and harsh reaction conditions; the plasma spray method has high equipment cost, complex operation, strong ultraviolet and electromagnetic radiation during the spraying process, and low material utilization rate; the electrochemical deposition method has low deposition efficiency when preparing the coating, the coating uniformity is difficult to control, the electrode design and electrolyte conditions are strict, the production cost is high, and it is difficult to achieve uniform deposition on substrates with complex shapes.

[0005] At present, there are few reports on the preparation of super-hydrophobic coatings on zinc alloy surfaces at home and abroad. The preparation of super-hydrophobic films currently has many shortcomings such as complex process, high energy consumption, and high equipment requirements. How to solve the problem of zinc alloy surface corrosion in the prior art has become the focus of the inventor's research. Summary of the invention

[0006] The present invention aims at the deficiencies in the prior art and provides a method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface, comprising the following steps: (1) zinc alloy surface pretreatment; (2) preparation of coating: the treated zinc alloy is vertically placed in a replacement solution and allowed to stand for a period of time, rinsed and then vertically placed in a growth solution and allowed to stand for a period of time, rinsed after taking out, then vertically placed in a constant temperature low surface energy solution and allowed to stand for a period of time, rinsed after taking out, and dried, i.e., a CoMIx coating with low surface energy is obtained on the zinc alloy surface. The above method adopts surface replacement and in-situ growth method to prepare a CoMIx coating with a lamellar structure on the zinc alloy surface, and the zinc alloy surface is modified by stearic acid low energy to obtain a super hydrophobic function. The method process involved in the present invention is simple, easy to control the reaction process, high production efficiency, low cost, improves the corrosion resistance and self-cleaning performance of the zinc alloy, and is conducive to realizing industrial production.

[0007] The present invention aims to develop a method for preparing a super-hydrophobic CoMIx coating on the surface of a zinc alloy, comprising the following steps: pre-treating the zinc alloy and ultrasonically cleaning it; then preparing a cobalt sulfate aqueous solution, preparing a cobalt coating on the surface of the zinc alloy by a static soaking process, then rinsing the sample with the cobalt coating on the surface with ionized water, placing it in an aqueous solution of a certain concentration of 2-methylimidazole, and standing for a period of time to obtain a CoMIx coating; finally, immersing the above sample in an anhydrous ethanol solution of stearic acid for chemical modification to reduce its surface energy, thereby obtaining a coating with super-hydrophobic properties. The above method enables the surface of the zinc alloy to have excellent super-hydrophobic properties, improves the corrosion resistance of the zinc alloy, and gives the zinc alloy self-cleaning properties, making up for the defects of the existing technology such as complex preparation process, high energy consumption, and high equipment requirements.

[0008] The specific modification principle of the present invention is as follows: Cobalt sulfate heptahydrate (CoSO4•7H2O) is often used as a drying agent for ceramic glazes and paints, and is also used in electroplating, alkaline batteries, the production of cobalt-containing pigments and other cobalt products, as well as catalysts, analytical reagents, feed additives, tire adhesives, and lead powder additives. Compared with other heavy metals, it has the advantages of low toxicity, high recyclability, and abundant resource reserves. In the present invention, cobalt ions are used to undergo a replacement reaction with zinc in zinc alloys to uniformly cover the surface of the zinc alloy, and a microscopic nanostructure is initially formed on the surface. 2-Methylimidazole (2-MI) is an intermediate for the manufacture of the drug metronidazole, and is also a curing agent for epoxy resins and other resins. It has the environmentally friendly characteristics of a wide source of raw materials, relatively low production costs, and less waste generated during the production process, and has good chemical stability and specific biological activity. In the present invention, the reaction of dimethylimidazole and divalent cobalt ions is used to improve the surface microstructure of the zinc alloy in one step, giving it superhydrophobicity and corrosion resistance.

[0009] The present invention provides a method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface, which specifically comprises the following steps: (1) Surface pretreatment of zinc alloy: After cutting the zinc alloy substrate, mechanically polish its surface with sandpaper, rinse and dry; (2) Preparation of coating: The treated zinc alloy is placed vertically in a replacement solution and allowed to stand for a period of time. After rinsing, it is placed vertically in a growth solution and allowed to stand for a period of time. After being taken out, it is rinsed. Then, it is placed vertically in a constant temperature low surface energy solution and allowed to stand for a period of time. After being taken out, it is rinsed and dried. Thus, a CoMIx coating with low surface energy is obtained on the surface of the zinc alloy.

[0010] Preferably, the zinc alloy in step (1) is Zn-0.5Mg-0.5Mn; the zinc alloy is cut into samples of 40mm×20mm×2mm, and its surface is mechanically polished using 240#, 800#, 1000#, and 1500# metallographic sandpaper in sequence, and then rinsed with deionized water and anhydrous ethanol in sequence to remove surface debris and oil stains, and then the sample is blown dry with cold air for use.

[0011] Preferably, the replacement solution in step (2) is an aqueous solution of cobalt sulfate heptahydrate, and the weight ratio of cobalt sulfate heptahydrate to deionized water is (1.6-2):50, which can ensure that the surface of the zinc alloy can be evenly covered with cobalt.

[0012] More preferably, in the replacement solution, the weight ratio of cobalt sulfate heptahydrate to deionized water is 2:50.

[0013] Preferably, the growth solution is an aqueous solution of 2-methylimidazole, and the mass ratio of 2-methylimidazole to deionized water is (1.5-2.5):50. Under the condition of consuming the least amount of chemicals, 2-methylimidazole can form a uniform complex with the cobalt element on the surface of the zinc alloy, so that the superhydrophobic property of the zinc alloy surface is optimized.

[0014] More preferably, in the growth solution, the mass ratio of 2-methylimidazole to deionized water is 2.2:50.

[0015] Preferably, the low surface energy solution is an anhydrous ethanol solution of stearic acid, and the molar concentration of stearic acid in the low surface energy solution is 0.030-0.035 mol / L; more preferably, the molar concentration of stearic acid in the low surface energy solution is 0.030 mol / L. Stearic acid, as a low surface energy substance, combines with the micro-nano surface to form a stable "air cushion", giving the zinc alloy super-hydrophobic properties.

[0016] Preferably, the working temperatures of the replacement solution and the growth solution are both room temperature, the immersion time in the replacement solution is 40-50 min; the immersion time in the growth solution is 90 min-120 min; the working temperature of the low surface energy solution is 45-50°C; the immersion time in the low surface energy solution is 2-3 h.

[0017] Preferably, the zinc alloy is washed with deionized water after being taken out of the replacement solution, rinsed with anhydrous ethanol after being taken out of the growth solution, and rinsed with anhydrous ethanol after being taken out of the low surface energy solution.

[0018] The preparation method has simple equipment and process, short reaction time, low surface energy of the coating surface, good hydrophobic effect and super hydrophobicity, good corrosion resistance and self-cleaning properties, and can extend the service life of the zinc alloy.

[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) After forming a cobalt layer on the surface of the zinc alloy, the present invention soaks it in a growth solution, grows it in situ, and modifies it with a low surface energy substance, so that the corrosive medium is not easy to approach the zinc alloy matrix, thereby significantly improving the corrosion resistance and self-cleaning performance of the zinc alloy surface and extending the service life of the zinc alloy.

[0020] (2) The surface replacement method and in-situ growth method adopted by the present invention have low reaction temperature, short reaction time, high efficiency, and are easy to promote and apply.

[0021] (3) The super-hydrophobic CoMIx coating obtained by this method requires simple equipment, and the preparation process is safe and convenient, especially compared with the hydrothermal reaction method, plasma spraying and electrochemical deposition method for preparing super-hydrophobic coatings.

[0022] (4) The present invention prepares a super-hydrophobic CoMIx layer on the surface of a zinc alloy, has no special requirements on the shape and size of the sample, has a simple surface pretreatment, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a microscopic SEM photo of the super-hydrophobic CoMIx coating on the zinc alloy surface prepared in Example 1; Figure 2 This is a static contact angle photograph of deionized water on the surface of the super-hydrophobic CoMIx coating in Example 1; Figure 3 The electrochemical impedance test comparison of the surface of the super-hydrophobic CoMIx coating prepared in Example 1 and the comparative example 1 without growth solution immersion; Figure 4 The electrochemical polarization curves of the super-hydrophobic CoMIx coating surface prepared in Example 1 are compared with those of Comparative Example 1. DETAILED DESCRIPTION

[0024] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The contact angle and rolling angle of the embodiment were measured using a static contact angle meter (SL200B). EIS tests were performed on a CS310H electrochemical workstation using 3.5wt% NaCl solution as the electrolyte. The test was performed at 0.01~10 5 The test was carried out in the frequency range of Hz with an AC amplitude of 10mV (vs.VOCP), and the impedance spectrum data view was finally fitted with Z. A 3.5wt%NaCl solution was used as the electrolyte for the potentiodynamic polarization curve test with a potential range of -0.15~0.65V (vs.VOCP).

[0026] All substances and reagents used, unless otherwise specified, were commercially available products.

[0027] The purpose of the present invention is to develop a method for preparing a super-hydrophobic CoMIx coating on a zinc alloy surface. To achieve the above purpose, the present invention uses a zinc alloy as a substrate, covers the surface of the zinc alloy with a layer of Co coating by an immersion replacement method, generates a CoMIx coating on the surface of the sample by an in-situ growth method, and then performs low-energy modification to prepare a super-hydrophobic CoMIx coating with a nano-sheet structure on the surface of the zinc alloy; the zinc alloys described below are all Zn-0.5Mg-0.5Mn.

[0028] The present invention will be further described below in conjunction with the embodiments and drawings.

[0029] Example 1 A method for preparing a low surface energy corrosion-resistant coating on a zinc alloy surface comprises the following steps:

[0030] (1) Surface pretreatment of zinc alloy: The zinc alloy substrate was cut into 40 mm × 20 mm × 2 mm specimens, and then the surface was mechanically polished using 240#, 800#, 1000#, and 1500# metallographic sandpapers in sequence. The specimens were rinsed with deionized water and anhydrous ethanol in sequence to remove the grinding debris and oil stains on the surface, and then the specimens were blown dry with cold air.

[0031] (2) Zinc surface replacement: Dissolve 2.0 g of cobalt sulfate heptahydrate in 50 ml of deionized water until fully dissolved. Place the sample in (1) vertically and completely immerse it. Let stand at room temperature for 45 min. After the reaction is complete, remove the sample and rinse it with deionized water.

[0032] (3) In situ growth of 2-methylimidazole: 2.2 g of 2-methylimidazole was dissolved in 50 ml of deionized water. The sample soaked in step (2) was then placed vertically and completely immersed. The sample was allowed to stand at room temperature for 1.5 h. After the reaction was complete, the sample was removed and rinsed with anhydrous ethanol.

[0033] (4) Surface low-energy modification: The zinc alloy with CoMIx coating obtained in step (3) was placed in a 45°C 0.03 mol / L stearic acid anhydrous ethanol solution for 2.5 h, and the sample was taken out and dried with cold air to obtain a super-hydrophobic coating with a micro-nano rough structure. The microscopic morphology of the obtained super-hydrophobic surface coating is shown in Figure 1 The contact angle of deionized water on the coating surface is 155.8° ( Figure 2 As shown), the rolling angle is 5°, as Figure 2 shown.

[0034] like Figure 3 As shown, the total impedance of the super hydrophobic coating zinc alloy prepared in Example 1 is 20900Ω•cm 2 , the corrosion resistance is significantly improved.

[0035] according to Figure 4 As shown, the polarization curve of the super-hydrophobic CoMIx coating prepared in Example 1 is located in the upper left relative to the coating zinc treated with no growth solution. Compared with Comparative Example 1, the corrosion potential of the super-hydrophobic coating shifts toward the positive potential direction, and the offset of the corrosion current is smaller, indicating that the super-hydrophobic coating has better corrosion resistance.

[0036] The prepared super-hydrophobic CoMIx coating is cleaned with water to remove dust on its surface without adhering to the super-hydrophobic coating itself, and has good self-cleaning performance.

[0037] Example 2 A method for preparing a low surface energy corrosion-resistant coating on a zinc alloy surface comprises the following steps:

[0038] (1) Surface pretreatment of zinc alloy: The zinc alloy substrate was cut into 40 mm × 20 mm × 2 mm specimens, and then the surface was mechanically polished using 240#, 800#, 1000#, and 1500# SiC sandpapers in sequence. The specimens were rinsed with deionized water and anhydrous ethanol in sequence to remove the grinding debris and oil stains on the surface, and then dried with cold air.

[0039] (2) Zinc surface replacement: Dissolve 2.0 g of cobalt sulfate heptahydrate in 50 ml of deionized water until fully dissolved. Place the sample in (1) vertically and completely immerse it. Let stand at room temperature for 40 min. After the reaction is complete, remove the sample and rinse it with deionized water.

[0040] (3) In situ growth of 2-methylimidazole: 1.5 g of 2-methylimidazole was dissolved in 50 ml of deionized water. The sample soaked in (2) was then placed vertically and completely immersed. The sample was allowed to stand at room temperature for 1.5 h. After the reaction was complete, the sample was removed and rinsed with anhydrous ethanol.

[0041] (4) Surface low-energy modification: The zinc alloy with CoMIx coating obtained in step (3) was placed in a 45°C 0.03 mol / L stearic acid anhydrous ethanol solution for 2.5 h, and the sample was taken out and dried with cold air to obtain a super hydrophobic coating with a micro-nano rough structure. The contact angle of deionized water on the coating surface was 156.8°, and the rolling angle was 4°. A super hydrophobic coating with a micro-nano rough structure was obtained.

[0042] The prepared super-hydrophobic CoMIx coating is cleaned with water to remove dust on its surface without adhering to the super-hydrophobic coating itself, and has good self-cleaning performance.

[0043] Example 3 A method for preparing a low surface energy corrosion-resistant coating on a zinc alloy surface comprises the following steps:

[0044] (1) Surface pretreatment of zinc alloy: The zinc alloy substrate was cut into 40 mm × 20 mm × 2 mm specimens, and then the surface was mechanically polished using 240#, 800#, 1000#, and 1500# SiC sandpapers in sequence. The specimens were rinsed with deionized water and anhydrous ethanol in sequence to remove the grinding debris and oil stains on the surface, and then dried with cold air.

[0045] (2) Zinc surface replacement: Dissolve 1.6 g of cobalt sulfate heptahydrate in 50 ml of deionized water until fully dissolved. Place the sample in (1) vertically and completely immerse it. Let it stand at room temperature for 50 min. After the reaction is complete, remove the sample and rinse it with deionized water.

[0046] (3) In situ growth of 2-methylimidazole: 2.0 g of 2-methylimidazole was added to 50 ml of deionized water to fully dissolve it. The sample soaked in (2) was then placed vertically and completely immersed. The sample was allowed to stand at room temperature for 2 h. After the reaction was completed, the sample was removed and rinsed with anhydrous ethanol.

[0047] (4) Surface low-energy modification: The zinc alloy with CoMIx coating obtained in step (3) was placed in a 50°C 0.03 mol / L stearic acid anhydrous ethanol solution for 2 h, and the sample was taken out and dried with cold air to obtain a super-hydrophobic coating with a micro-nano rough structure. The contact angle of deionized water on the coating surface was 153.6°, and the rolling angle was 7°. A super-hydrophobic coating with a micro-nano rough structure was obtained.

[0048] The prepared super-hydrophobic CoMIx coating is cleaned with water to remove dust on its surface without adhering to the super-hydrophobic coating itself, and has good self-cleaning performance.

[0049] Comparative Example 1 A method for preparing a low surface energy corrosion-resistant coating on a zinc alloy surface comprises the following steps:

[0050] (1) Surface pretreatment of zinc alloy: The zinc alloy substrate was cut into 40 mm × 20 mm × 2 mm specimens, and then the surface was mechanically polished using 240#, 800#, 1000#, and 1500# metallographic sandpapers in sequence. The specimens were rinsed with deionized water and anhydrous ethanol in sequence to remove the grinding debris and oil stains on the surface, and then dried with cold air.

[0051] (2) Zinc surface replacement: Dissolve 2.0 g of cobalt sulfate heptahydrate in 50 ml of deionized water until fully dissolved. Place the sample in (1) vertically and completely immerse it. Let stand at room temperature for 45 min. After the reaction is complete, remove the sample and rinse it with deionized water.

[0052] (3) Surface low-energy modification: The zinc alloy with a Co coating on the surface obtained in step (2) was placed in a 45°C 0.03 mol / L stearic acid anhydrous ethanol solution for 2.5 h. After taking it out, the sample was taken out and dried with cold air to obtain a superhydrophobic coating with a micro-nano rough structure.

[0053] The contact angle of deionized water on the coating surface is 138°, and the rolling angle is greater than 60°.

[0054] The prepared Co coating was cleaned with water to remove dust on its surface. The adhesion between water and the coating was strong and the self-cleaning performance was poor.

[0055] It can be seen that the contact angle of comparative example 1 is about 143°, which is significantly smaller than that of embodiments 1-3, and the rolling angle is significantly larger than that of embodiments 1-3, which does not meet the super-hydrophobic requirements, indicating that the hydrophobic properties of the coatings obtained in embodiments 1-3 are significantly better than those of comparative example 1, proving that the in-situ growth of 2-methylimidazole in the present invention can significantly improve the nano-microscopic morphology of the substrate surface, thereby improving the super-hydrophobic properties.

[0056] Experimental example The coating was electrochemically tested using an electrochemical station. The working electrode was a Zn-0.5Mg-0.5Mn alloy surface coating, the reference electrode was a saturated calomel electrode, the auxiliary electrode was a platinum sheet, and the electrolyte was a 3.5% sodium chloride solution. The electrochemical AC impedance method was used to test the corrosion resistance of the coating surface. The impedance arc represents the corrosion resistance of the coating. The larger the impedance arc, the better the corrosion resistance.

[0057] After fitting by Origin software, Figure 3As shown, the impedance modulus of the zinc alloy prepared in Comparative Example 1 that has not been immersed in the growth solution is 1030Ω•cm² at maximum, and the total impedance of the coated zinc alloy in Example 1 that has been immersed in the growth solution is 20900Ω•cm². Compared with Comparative Example 1, the coating of the present invention significantly improves the corrosion resistance of the zinc alloy in Example 1.

[0058] according to Figure 4 As shown, compared with the electrochemical polarization curve of the surface of the super-hydrophobic CoMIx coating prepared in Example 1 and that of Comparative Example 1, the polarization curve of the CoMIx coating is located at the upper left of the polarization curve of Comparative Example 1, and compared with Comparative Example 1, the corrosion potential of the super-hydrophobic coating shifts toward the positive potential direction, and the offset of the corrosion current is smaller, indicating that the super-hydrophobic CoMIx coating prepared in Example 1 has better corrosion resistance.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any equivalent substitutions, modifications, etc. made by technicians in this field without any creative work within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface, characterized in that: The steps include: (1) Surface pretreatment of zinc alloy: After cutting the zinc alloy substrate, mechanically polish its surface with sandpaper, rinse and dry; (2) Preparation of coating: The treated zinc alloy is placed vertically in a replacement solution and allowed to stand for a period of time. After rinsing, it is placed vertically in a growth solution and allowed to stand for a period of time. After being taken out, it is rinsed. Then, it is placed vertically in a constant temperature low surface energy solution and allowed to stand for a period of time. After being taken out, it is rinsed and dried. Thus, a CoMIx coating with low surface energy is obtained on the surface of the zinc alloy.

2. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The zinc alloy in step (1) is Zn-0.5Mg-0.5Mn; the zinc alloy is cut into samples of 40mm×20mm×2mm, and its surface is mechanically polished using 240#, 800#, 1000#, and 1500# metallographic sandpaper in sequence, and then rinsed with deionized water and anhydrous ethanol in sequence to remove surface debris and oil stains, and then the sample is blown dry with cold air for use.

3. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The replacement solution in step (2) is an aqueous solution of cobalt sulfate heptahydrate, and the weight ratio of cobalt sulfate heptahydrate to deionized water is (1.6-2):

50.

4. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 3, characterized in that: In the replacement solution, the weight ratio of cobalt sulfate heptahydrate to deionized water is 2:

50.

5. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The growth solution is an aqueous solution of 2-methylimidazole, and the mass ratio of 2-methylimidazole to deionized water is (1.5-2.5):

50.

6. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 5, characterized in that: The mass ratio of 2-methylimidazole to deionized water is 2.2:

50.

7. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The low surface energy solution is an anhydrous ethanol solution of stearic acid, and the molar concentration of stearic acid in the low surface energy solution is 0.030-0.035 mol / L.

8. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 7, characterized in that: The molar concentration of stearic acid in the low surface energy solution is 0.030 mol / L.

9. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The working temperatures of the replacement solution and the growth solution are both room temperature, the immersion time in the replacement solution is 40-50 minutes; the immersion time in the growth solution is 90 minutes to 120 minutes; the working temperature of the low surface energy solution is 45-50°C; the immersion time in the low surface energy solution is 2-3 hours.

10. The method for preparing a low surface energy corrosion-resistant super hydrophobic coating on a zinc alloy surface according to claim 1, characterized in that: The zinc alloy was washed with deionized water after being taken out of the replacement solution, rinsed with anhydrous ethanol after being taken out of the growth solution, and rinsed with anhydrous ethanol after being taken out of the low surface energy solution.