Fe-Cr-Si alloy with corrosion-resistant passive film and preparation method
By designing the Fe-Cr-Si alloy components and arc smelting and electrolyzing preparation under high vacuum environment, dense Cr and Si oxide passivation films are formed, which solves the high cost of high-temperature preparation of oxide films and poor performance in the current technology. The problem of this achieves low cost, simple process and high corrosion resistance.
Patent Information
- Application Number
- CN202411240699.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-28
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is costly and complex when preparing oxide films under high temperature environments, and it is difficult to prepare a passivation film with corrosion resistance at room temperature, especially in harsh corrosion environments.
By designing the components of Fe-Cr-Si alloys are Fe 66% to 76%, Cr 18% to 22%, Si 6% to 12%, arc melting under high vacuum environment and electrolyzing in hydrochloric acid electrolyte, the main formation is formed A dense passivation film composed of oxides of Cr and Si.
It realizes the preparation of a corrosion-resistant passivation film with low cost and simple process at room temperature, which can maintain good performance under a strong corrosion environment, and the density of the passivation film is increased by at least 30mV/SCE, meeting the requirements of harsh corrosion environments.
Smart Images

Figure CN119082829A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an alloy and a preparation method thereof, in particular to a Fe-Cr-Si alloy with a corrosion-resistant passivation film and a preparation method thereof. Background Art
[0002] Many metal components in chemical environments are subject to harsh service conditions and work under adverse conditions for a long time. They fail due to corrosion, which causes the degradation of material performance and even leads to economic losses in severe cases. Therefore, it is particularly important to develop materials suitable for working under such working conditions.
[0003] By adding passivating elements in a reasonable manner, the corrosion behavior of materials in a corrosive environment can be slowed down or prevented. For example, materials containing Cr and Si elements will be oxidized in the air to form an oxide film, thereby preventing oxygen from further contacting the elements on the surface of the metal or alloy and causing an oxidation reaction, so that the surface of such metal or alloy is converted into a state that is not easily oxidized.
[0004] The use of coating technology can improve the corrosion resistance of the alloy surface, but the coating process is complicated and generally pollutes the environment. In high-temperature environments, the coating will diffuse with the substrate, which may even cause the coating to fail in severe cases. In addition, the complexity of the equipment will inevitably increase the cost. Oxidation treatment at high temperature to obtain an oxide film is also one of the methods to improve the corrosion resistance of the alloy surface, but the reaction conditions are harsh and high-temperature equipment is required. In addition, if there are some elements in the alloy whose thermal expansion coefficient does not match the substrate, the use of high temperature to prepare the oxide film will produce thermal stress and cause the oxide film to crack, destroying its integrity and greatly reducing its performance.
[0005] Therefore, it is necessary to provide a method for preparing a passivation film at room temperature, which can meet the service requirements in a strong corrosive environment while having a simple preparation process and low preparation cost. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a low-cost Fe-Cr-Si alloy with a corrosion-resistant passivation film; the present invention also provides a method for preparing the Fe-Cr-Si alloy with a corrosion-resistant passivation film with a simple process.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a passivation film is provided on the surface of the Fe-Cr-Si alloy; the composition and mass fraction of the Fe-Cr-Si alloy are: Fe 66% to 76%, Cr 18% to 22%, and Si 6% to 12%.
[0008] Furthermore, the main components of the passivation film are oxides of Cr and Si, and the mass fraction of the oxides is greater than 77%.
[0009] The composition design concept of the present invention is as follows: according to Tamman's law: when the Cr / Fe atoms are 1 / 8 or 1 / 4, the higher the Cr content, the better the corrosion resistance of the alloy; by adding Si elements to the alloy, it is possible to ensure that a stable oxide is formed in a corrosive environment. The present invention reasonably controls the amount of alloy added to ensure that the alloy can form a continuous and dense anti-corrosion passivation film during the polarization process.
[0010] The method of the present invention adopts the following steps: 1) smelting to obtain Fe-Cr-Si alloy according to the composition design of Fe-Cr-Si alloy; 2) cleaning the surface of the Fe-Cr-Si alloy; 3) The Fe-Cr-Si alloy after surface cleaning is electrolyzed in an electrolyte to form a passivation film on the Fe-Cr-Si alloy.
[0011] Furthermore, in step 3), the electrolyte is a hydrochloric acid electrolyte with a concentration of 0.3 to 0.8 mol / L.
[0012] Furthermore, in step 3), the polarization potential of the electrolysis process is -1.0 V / SCE to 2 V / SCE.
[0013] Furthermore, the passivation range of the electrolysis process is -0.16 to 0.91 V / SCE.
[0014] Furthermore, the polarization time of the electrolysis process is 20 minutes to 35 minutes.
[0015] Furthermore, in the electrolysis process, the Fe-Cr-Si alloy is first allowed to stand at an open circuit potential for 20 to 30 minutes and then polarized.
[0016] The beneficial effects of adopting the above technical scheme are: the present invention is based on component design, and by reasonably regulating the amount of alloy added, it is ensured that a continuous and dense corrosion-resistant passivation film can be formed on the alloy surface during the polarization process; the present invention has good corrosion resistance, can meet the needs of a strong corrosion environment, and its preparation process is simple, the equipment requirements are low, the preparation cost is low and the performance is excellent.
[0017] The method of the present invention uses reasonable component design and arc melting process to prepare Fe-Cr-Si alloy in a high vacuum environment, cleans the alloy surface, and electrolyzes in an electrolyte to obtain a Fe-Cr-Si alloy with a corrosion-resistant passivation film; the preparation process is simple, the preparation cost is low, and the equipment requirements are low. The method of the present invention adopts an electrolysis process in an acidic electrolyte, and controls the density of the passivation film by controlling the alloy composition, electrolyte and voltage, so that the prepared passivation film alloy has a wider passivation range than the passivation film naturally formed by stainless steel, and the corrosion potential is increased by at least 30mV / SCE; the main components of the obtained passivation film are Cr and Si oxides, with a mass fraction content of more than 77%, and the corrosion resistance is significantly improved, which can meet the environment with strong corrosion ability. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0019] Figure 1 is a morphology diagram of the passivation film obtained in Example 1 of the present invention; Figure 2 is a morphology diagram of the passivation film obtained in Example 2 of the present invention; Figure 3 is the morphology of the passivation film obtained in the comparative example; Figure 4 1 is a dynamic point potential polarization curve diagram of the passivation film obtained in the embodiment of the present invention and the comparative example; Figure 5 It is the full XPS spectrum of the passivation film obtained in the embodiment of the present invention. DETAILED DESCRIPTION
[0020] The Fe-Cr-Si alloy with corrosion-resistant passivation film is designed based on the composition. By reasonably adjusting the amount of alloy added, it is ensured that a continuous and dense corrosion-resistant passivation film can be formed on the alloy surface during the polarization process. Since Cr and Si elements have a higher affinity for oxygen than Fe, they are easy to combine with oxygen preferentially to form protective Cr2O3 and SiO2 oxide films in a corrosive environment, effectively slowing down or preventing oxidation. In a corrosive environment, when the elements in the alloy diffuse, if the content of Cr and Si in the alloy is small, it will lead to the failure to form a continuous oxide film on the alloy surface; or when the alloy composition design is unreasonable, firstly, excessive alloy elements will greatly increase the cost, and secondly, when the amount of element addition exceeds a certain limit, it may reduce the corrosion resistance of the alloy (due to unreasonable regulation of alloy elements, the passivation film will crack or peel off, affecting the integrity of the passivation film). Therefore, the actual application environment must be fully combined in the alloy composition design. The composition and mass fraction of the Fe-Cr-Si alloy are: Fe 66%~76%, Cr 18%~22%, Si 6%~12%.
[0021] The preparation method of the Fe-Cr-Si alloy with a corrosion-resistant passivation film adopts the following steps: 1) Melting: According to the composition design of Fe-Cr-Si alloy, Fe-Cr-Si alloy is melted. The melting process first washes the furnace and then performs arc melting; the furnace washing process is: put the raw materials into the arc furnace according to the designed ratio, evacuate the arc furnace to a vacuum degree of less than or equal to 1.9E1Pa, that is, less than or equal to 19Pa, and then fill it with argon gas to a vacuum degree of -0.075MPa to -0.06MPa for furnace washing; the arc melting process is: evacuate to a vacuum degree of 8E-3 to 9E-3Pa, arc melt at 1550 to 1680℃ for 5 to 6 minutes, and turn the furnace over for 6 times or more to ensure uniform composition, and obtain Fe-Cr-Si alloy.
[0022] 2) Surface cleaning: The Fe-Cr-Si alloy is surface cleaned, and the surface cleaning process is: the Fe-Cr-Si alloy obtained by smelting is first polished with sandpaper and then polished with a polishing agent. It is best to first polish it with sandpaper with particle sizes from low to high to 2000 mesh, then polish it with a 2.5um polishing agent, and finally ultrasonically clean it with anhydrous ethanol and blow it dry.
[0023] 3) Passivation treatment: The Fe-Cr-Si alloy after surface cleaning is electrolyzed in an electrolyte to form a passivation film on the surface of the Fe-Cr-Si alloy. The electrolysis process is as follows: a hydrochloric acid electrolyte with a concentration of 0.3-0.8 mol / L is used; after the alloy is placed in the electrolyte, the reference electrode is a saturated calomel electrode (SCE), the auxiliary electrode is a Pt electrode, and the working electrode is an alloy sample; the alloy is first allowed to stand at an open circuit potential for 20-30 minutes; and then polarized, the polarization potential is -1.0V / SCE-2V / SCE, the scanning rate is 1-3mv / s, preferably 2mv / s, the polarization time is 20min-35min, and the passivation interval for forming a passivation film is -0.16-0.91V / SCE.
[0024] 4) After adopting the above method, the main components of the formed passivation film are Cr oxide and Si oxide, and the total mass fraction of these two oxides in the passivation film is greater than 77%.
[0025] Example 1: The Fe-Cr-Si alloy with a corrosion-resistant passivation film and its preparation method are described as follows.
[0026] 1) Melting: The composition and mass fraction of the Fe-Cr-Si alloy are as follows: Fe 70%, Cr 20%, Si 10%. The prepared raw materials are placed in an electric arc furnace according to the above ratio, the electric arc furnace is evacuated to a vacuum degree of 16Pa, and then filled with argon gas to a vacuum degree of -0.075MPa for furnace cleaning, and then evacuated to a vacuum degree of 9E-3Pa, arc-melted at 1550-1600℃ for 5min, and turned over and melted 8 times to obtain a Fe-Cr-Si alloy.
[0027] 2) Surface treatment: The Fe-Cr-Si alloy obtained by smelting was polished to 2000 mesh with sandpaper of increasing particle size, then polished with 2.5um polishing agent, ultrasonically cleaned with anhydrous ethanol and blown dry.
[0028] 3) Passivation treatment: The alloy was placed in a 0.3 mol / L hydrochloric acid electrolyte and allowed to stand at an open circuit potential for 20 min; then polarization was performed at a polarization potential of -1.0 V / SCE to 2 V / SCE, a scanning rate of 2 mv / s, and a polarization time of 35 min to obtain a Fe-Cr-Si alloy with a corrosion-resistant passivation film.
[0029] 4) The morphology of the passivation film obtained in this embodiment is shown in Figure 1 , it can be seen that the passivation film maintains good integrity and does not crack; the dynamic point potential polarization curve of the passivation film obtained in this embodiment is shown in Figure 4 It can be seen that the passivation range is -0.16 to 0.90 V / SCE, and the corrosion potential is -0.196 V / SCE; the XPS full spectrum of the passivation film obtained in this embodiment is shown in Figure 5 It can be seen that the main components of the passivation film are oxides of Cr and Si. After fitting calculation, it is known that the mass fraction is 81%, and the corrosion resistance is significantly improved, which can meet the environment with strong corrosion ability.
[0030] Example 2: The Fe-Cr-Si alloy with a corrosion-resistant passivation film and its preparation method are described as follows.
[0031] 1) Melting: The composition and mass fraction of the Fe-Cr-Si alloy are as follows: Fe 68%, Cr 20%, Si 12%. The prepared raw materials are placed in an electric arc furnace according to the above ratio, the electric arc furnace is evacuated to a vacuum degree of 19Pa, and then filled with argon gas to a vacuum degree of -0.070MPa for furnace cleaning, and then evacuated to a vacuum degree of 9E-3Pa, arc-melted at 1600-1650°C for 6min, and turned over and melted 7 times to obtain a Fe-Cr-Si alloy.
[0032] 2) Surface treatment: The Fe-Cr-Si alloy obtained by smelting was polished to 2000 mesh with sandpaper of increasing particle size, then polished with 2.5um polishing agent, ultrasonically cleaned with anhydrous ethanol and blown dry.
[0033] 3) Passivation treatment: The alloy was placed in a 0.5 mol / L hydrochloric acid electrolyte and allowed to stand at an open circuit potential for 30 min; then polarization was performed at a polarization potential of -1.0 V / SCE to 2 V / SCE, a scanning rate of 2 mv / s, and a polarization time of 20 min to obtain a Fe-Cr-Si alloy with a corrosion-resistant passivation film.
[0034] 4) The morphology of the passivation film obtained in this embodiment is shown in Figure 2 , it can be seen that the passivation film maintains good integrity and does not crack; the dynamic point potential polarization curve of the passivation film obtained in this embodiment is shown in Figure 4 It can be seen that the passivation range is -0.17 to 0.91 V / SCE, and the corrosion potential is 0.194 V / SCE; the XPS full spectrum of the passivation film obtained in this embodiment is shown in Figure 5 It can be seen that the main components of the passivation film are oxides of Cr and Si. After fitting calculation, it is known that the mass fraction content is 82%, and the corrosion resistance is significantly improved, which can meet the environment with strong corrosion ability.
[0035] Example 3: The Fe-Cr-Si alloy with a corrosion-resistant passivation film and its preparation method are described as follows.
[0036] 1) Melting: The composition and mass fraction of the Fe-Cr-Si alloy are as follows: Fe 66%, Cr 22%, Si 6%. The prepared raw materials are placed in an electric arc furnace according to the above ratio, the electric arc furnace is evacuated to a vacuum degree of 18Pa, and then filled with argon gas to a vacuum degree of -0.060MPa for furnace cleaning, and then evacuated to a vacuum degree of 9E-3Pa, arc-melted at 1630-1680°C for 5.5min, and turned over and melted 7 times to obtain a Fe-Cr-Si alloy.
[0037] 2) Surface treatment: The Fe-Cr-Si alloy obtained by smelting was polished to 2000 mesh with sandpaper of increasing particle size, then polished with 2.5um polishing agent, ultrasonically cleaned with anhydrous ethanol and blown dry.
[0038] 3) Passivation treatment: The alloy was placed in a 0.8 mol / L hydrochloric acid electrolyte and allowed to stand at an open circuit potential for 25 min; then polarization was performed at a polarization potential of -1.0 V / SCE to 2 V / SCE, a scanning rate of 1 mv / s, and a polarization time of 30 min to obtain a Fe-Cr-Si alloy with a corrosion-resistant passivation film.
[0039] 4) The passivation film obtained in this embodiment maintains good integrity without cracks; the main components of the passivation film are oxides of Cr and Si, and the mass fraction of the two in the passivation film is 83%, and the corrosion resistance is significantly improved, which can meet the requirements of environments with strong corrosion ability.
[0040] Example 4: The Fe-Cr-Si alloy with corrosion-resistant passivation film and its preparation method are described as follows.
[0041] 1) Melting: The composition and mass fraction of the Fe-Cr-Si alloy are as follows: Fe 72%, Cr 18%, Si 10%. The prepared raw materials are placed in an electric arc furnace according to the above ratio, the electric arc furnace is evacuated to a vacuum degree of 15Pa, and then filled with argon gas to a vacuum degree of -0.065MPa for furnace cleaning, and then evacuated to a vacuum degree of 9E-3Pa, arc-melted at 1580-1630℃ for 5.5min, and turned over and melted 8 times to obtain a Fe-Cr-Si alloy.
[0042] 2) Surface treatment: The Fe-Cr-Si alloy obtained by smelting was polished to 2000 mesh with sandpaper of increasing particle size, then polished with 2.5um polishing agent, ultrasonically cleaned with anhydrous ethanol and blown dry.
[0043] 3) Passivation treatment: The alloy was placed in a 0.6 mol / L hydrochloric acid electrolyte and allowed to stand at an open circuit potential for 28 min; then polarization was performed at a polarization potential of -1.0 V / SCE to 2 V / SCE, a scan rate of 3 mv / s, and a polarization time of 25 min to obtain a Fe-Cr-Si alloy with a corrosion-resistant passivation film.
[0044] 4) The passivation film obtained in this embodiment maintains good integrity without cracks; the main components of the passivation film are oxides of Cr and Si, and the mass fraction of the two in the passivation film is 79%, and the corrosion resistance is significantly improved, which can meet the environment with strong corrosion ability.
[0045] Comparative Example: This comparative example is based on the Fe-Cr-Si alloy, increases its Si content, and adopts this method to prepare it to verify whether it is feasible.
[0046] 1) The composition and mass fraction of the Fe-Cr-Si alloy in this comparative example are as follows: Fe 67%, Cr 20%, Si 13%. The preparation method adopts the process parameters described in the above embodiment 1.
[0047] 2) The morphology of the passivation film obtained in this comparative example is shown in Figure 3 ,Depend on Figure 3 It can be seen that due to the increase in Si content in the alloy, cracking was induced by stress during the formation of the passivation film. The dynamic point potential polarization curves of the passivation films obtained in Examples 1 and 2 and the comparative example are shown in Figure 4 ,Depend on Figure 4It can be seen that Example 1 is improved by at least 30 mV / SCE compared with -0.230 V / SCE of the comparative example, and Example 2 is improved by at least 30 mV / SCE compared with -0.230 V / SCE of the comparative example, indicating that the passivation film prepared in the examples has higher corrosion resistance.
Claims
1. A Fe-Cr-Si alloy having a corrosion-resistant passivation film, characterized in that: The Fe-Cr-Si alloy has a passivation film on its surface; the composition and mass fraction of the Fe-Cr-Si alloy are: Fe 66% to 76%, Cr 18% to 22%, and Si 6% to 12%.
2. The Fe-Cr-Si alloy with a corrosion resistant passive film according to claim 1, characterized in that: The main components of the passivation film are oxides of Cr and Si, and the mass fraction of the oxides is greater than 77%.
3. The method for preparing the Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 1 or 2, characterized in that: The following steps are adopted: 1) according to the composition design of Fe-Cr-Si alloy, smelting to obtain Fe-Cr-Si alloy; 2) cleaning the surface of the Fe-Cr-Si alloy; 3) The Fe-Cr-Si alloy after surface cleaning is electrolyzed in an electrolyte to form a passivation film on the Fe-Cr-Si alloy.
4. The method for preparing a Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 3, characterized in that: In the step 3), the electrolyte is a hydrochloric acid electrolyte with a concentration of 0.3 to 0.8 mol / L.
5. The method for preparing a Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 3 or 4, characterized in that: In the step 3), the polarization potential of the electrolysis process is -1.0 V / SCE to 2 V / SCE.
6. The method for preparing a Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 6, characterized in that: The passivation range of the electrolysis process is -0.16 to 0.91 V / SCE.
7. The method for preparing a Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 5, characterized in that: The polarization time of the electrolysis process is 20 minutes to 35 minutes.
8. The method for preparing a Fe-Cr-Si alloy having a corrosion resistant passivation film according to claim 7, characterized in that: In the electrolysis process, the Fe-Cr-Si alloy is first allowed to stand at an open circuit potential for 20 to 30 minutes and then polarized.