Functional fiber reinforcement, composite material and preparation method of functional fiber reinforcement

By using functional fiber reinforcement in the vacuum introduction process and using linear phenolic fibers as the curing agent of epoxy resin to participate in the reaction, the flame retardant performance of composite materials in the field of rail transit is solved, and the problems of inlet blockage of the introduction port are achieved efficiently Structural flame retardant and industrial production.

CN119082983AActive Publication Date: 2024-12-06HENGSHEN
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411386827.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06
Estimated Expiration
2044-09-30

AI Technical Summary

Technical Problem

The resin used in composite materials in the existing vacuum introduction process lacks flame retardant properties, which makes it difficult to achieve the flame retardant requirements of EN45545-2 in the field of rail transit, and the addition of flame retardant powder will lead to settlement and inlet blockage.

Method used

Using functional fiber reinforcement bodies, including carbon fiber and linear phenolic fibers, the linear phenolic fibers are introduced into the carbon fiber fabric in the form of a braided fabric. After melting, the linear phenolic fibers participate in the reaction as a curing agent for epoxy resin to improve flame retardant performance, and The high-temperature curing reaction is participated in the linear phenolic resin and anhydride curing agent introduced into the resin system in vacuum.

Benefits of technology

Structural flame retardant in the vacuum introduction process is realized, reaching the highest flame retardant level HL3 in EN45545-2, overcoming the dilemma of the inability to effectively introduce one-way tows, and simplifying the preparation process of composite materials, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082983A_ABST
    Figure CN119082983A_ABST
Patent Text Reader

Abstract

The invention discloses a functional fiber reinforcement, a composite material and a preparation method thereof, and belongs to the technical field of composite materials. The functional fiber reinforcement comprises carbon fibers and linear phenolic fibers; the linear phenolic fiber is prepared from the following raw materials: a toughening system, boric acid and first linear phenolic resin in a mass ratio of (10-30): (0.8-1): (69.2-89). The functional fiber reinforcement can be effectively combined with a flame-retardant resin system for vacuum infusion, structural flame retardance is achieved, the charring characteristic in the combustion process is improved, and the highest flame retardant grade HL3 of R1 in EN45545-2 is achieved under the condition that the rear-end infusion technology is not affected. Through introduction of the functional fiber reinforcement, the defects of a woven fabric reinforcement and a warp knitting fabric reinforcement can be ingeniously overcome, and the problem that a one-way tow cannot be effectively introduced in vacuum is solved. The corresponding preparation method of the composite material is simple and easy to operate, and industrial production can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a functional fiber reinforcement, a composite material and a preparation method thereof. Background Art

[0002] The vacuum infusion molding process is a composite material molding process that uses vacuum negative pressure as power to achieve resin introduction, fiber impregnation, and resin curing. Its main features are low cost, low product porosity, small impact on the environment, performance close to that of the autoclave process, and suitability for the manufacture of large structures. It is widely recognized in the fields of construction, automobiles, rail transit, and wind power.

[0003] At present, most of the resins used in the vacuum introduction process are unsaturated polyester and epoxy resin, which do not have flame retardant properties. In order to meet the increasingly high flame retardant requirements in the fields of construction, automobiles, rail transit, and wind power, especially the EN45545-2 flame retardant requirements proposed in the field of rail transit, this standard is the most stringent and most fully classified standard in the field of rail transit flame retardant, and has strict requirements on various aspects of flame retardant such as flame spread, combustion heat release, smoke density (4min), and smoke concentration. At present, most of the flame retardant requirements are achieved by adding a large amount of flame retardant powders, such as aluminum hydroxide, magnesium hydroxide, zinc borate, magnesium silicate, ammonium polyphosphate, melamine urate, etc. These solutions are mostly suitable for prepreg resin systems, but because it is a vacuum introduction resin system, the basic requirement is that the viscosity is less than 600cps at 25°C. When a low-viscosity flame retardant resin system with a large amount of flame retardant powder is added, there will be a problem of sedimentation of the flame retardant in the resin system, and the inlet will be blocked due to sedimentation. In addition, when flame-retardant liquid resin is impregnated with multiple layers of continuous fibers under negative pressure, the flame-retardant powder is intercepted by the fibers during the flow of low-viscosity (below 600cps) resin, forming a blocking layer, which brings defects to the vacuum introduction process, such as surface dry spots and delamination.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a functional fiber reinforcement, a composite material and a preparation method thereof, so as to solve or improve the above technical problems.

[0006] The present invention can be implemented like this:

[0007] In a first aspect, the present invention provides a functional fiber reinforcement, the functional fiber reinforcement comprising carbon fiber and linear phenolic fiber; the functional fiber reinforcement is obtained by mixing the carbon fiber and the linear phenolic fiber;

[0008] Among them, the raw materials for preparing linear phenolic fiber include a toughening system, boric acid and a first linear phenolic resin in a mass ratio of (10-30):(0.8-1):(69.2-89); the toughening system includes at least one of nylon block copolymer, polypropylene, polyether sulfone and polyaryletherketone.

[0009] In an optional embodiment, the linear phenolic fiber has at least one of the following characteristics:

[0010] Feature 1: Particle size D of the toughening system 90 ≤90μm;

[0011] Feature 2: The melting point of the first linear phenolic resin is 95°C to 120°C;

[0012] Feature 3: The diameter of the linear phenolic fiber is 12 μm to 14 μm.

[0013] In an optional embodiment, the functional fiber reinforcement includes warp direction fibers and weft direction fibers, wherein the warp direction fibers are carbon fiber bundles and the weft direction fibers are linear phenolic fibers;

[0014] In an optional embodiment, the mixed weaving form includes a plain 1 / 1 form, a twill 2 / 2 form, a twill 3 / 1 form, a satin 5S form or a satin 8S form.

[0015] In an alternative embodiment, the weaving form is a twill 2 / 2 form or a twill 3 / 1 form.

[0016] In an optional embodiment, the total amount of carbon fiber tows in the functional fiber reinforcement is 3,000 to 50,000; and / or the total amount of linear phenolic fiber tows is 1,500 to 6,000.

[0017] In a second aspect, the present invention provides a composite material, wherein raw materials for preparing the composite material include a flame retardant resin system for vacuum introduction and a functional fiber reinforcement according to any one of the aforementioned embodiments.

[0018] In an optional embodiment, the mass ratio of the flame retardant resin system for vacuum introduction to the functional fiber reinforcement is 3.5:6.5 to 4.5:5.5.

[0019] In an optional embodiment, the flame retardant resin system for vacuum introduction includes an epoxy resin component, a flame retardant resin component, a toughening resin component and a curing agent component.

[0020] In an optional embodiment, the mass ratio of the epoxy resin component, the flame retardant resin component, the toughening resin component and the curing agent component is (49-51):(14-18):10:(23-25).

[0021] In an optional embodiment, the flame retardant resin system for vacuum introduction has a viscosity of 400 cps to 1200 cps at 25°C.

[0022] In an optional embodiment, the epoxy resin component includes an epoxy resin; the epoxy resin includes at least one of a bisphenol A epoxy resin and a bisphenol F epoxy resin.

[0023] In an alternative embodiment, the epoxy resin component further comprises an epoxy reactive diluent.

[0024] In an alternative embodiment, the bisphenol A epoxy resin includes at least one of E-51 liquid resin, E-54 liquid resin, E-44 liquid resin, and NPEL127 liquid resin.

[0025] In an alternative embodiment, the bisphenol F epoxy resin comprises NPEF-170 epoxy resin.

[0026] In an alternative embodiment, the epoxy reactive diluent includes at least one of XY622, XY699 and XY678.

[0027] In an alternative embodiment, the flame retardant resin component includes at least one of a second phenolic novolac resin and a phosphorus-containing epoxy resin.

[0028] In an alternative embodiment, the melting point of the second phenolic linear resin is 60°C to 80°C.

[0029] In an optional embodiment, the phosphorus-containing epoxy resin includes at least one of a phosphate-modified phosphorus-containing epoxy resin and a DOPO-modified phosphorus-containing epoxy resin.

[0030] In an optional embodiment, the phosphorus-containing epoxy resin modified by phosphate ester includes at least one of FR-633 and FR-7016.

[0031] In an alternative embodiment, the DOPO-modified phosphorus-containing epoxy resin includes at least one of D200, D201 and D202.

[0032] In an optional embodiment, the toughening resin component includes at least one of a polyurethane-modified epoxy resin, a terminal carboxyl-modified nitrile rubber resin, a dimer acid-modified epoxy resin, and a core-shell particle toughening resin containing nano rubber particles.

[0033] In an alternative embodiment, the polyurethane-modified epoxy resin includes EPU133.

[0034] In an optional embodiment, the carboxyl-terminated nitrile rubber resin includes at least one of CTBN1300X13, CTBN1300X8 and CTBN1300X31.

[0035] In an alternative embodiment, the dimer acid-modified epoxy resin includes at least one of HyPox DA323 and YD-172.

[0036] In an optional embodiment, the core-shell particle toughening resin containing nano rubber particles includes at least one of MX-962, MX-150 and MX-160.

[0037] In an optional embodiment, the curing agent component includes at least one of a liquid anhydride curing agent and a modified liquid anhydride curing agent.

[0038] In an optional embodiment, the curing agent component further includes a liquid accelerator.

[0039] In an alternative embodiment, the modified liquid anhydride curing agent includes YEG-1070.

[0040] In an optional embodiment, the liquid accelerator includes at least one of an imidazole-modified liquid accelerator and a complex-type liquid modifier.

[0041] In an optional embodiment, the imidazole-modified liquid accelerator includes at least one of 2E4MZ-CN and 2PHZ-CN.

[0042] In an alternative embodiment, the complex-type liquid modifier includes at least one of Anchor 1170, Anchor 1171, Anchor 1053, and Anchor 1115.

[0043] In a third aspect, the present invention provides a method for preparing a composite material as described in any of the aforementioned embodiments, comprising the following steps: vacuum introducing a preform made of functional fiber reinforcement and a flame retardant resin system for vacuum introduction, keeping the preform warm at 95°C to 120°C for 1h to 3h, and then curing the preform at 130°C to 150°C.

[0044] In an optional embodiment, the preparation of the preform includes: laying the functional fiber reinforcement in a preset laying direction, and maintaining the pressure under negative pressure at 90° C. to 100° C. for 20 min to 30 min.

[0045] The beneficial effects of the present invention include:

[0046] The functional fiber reinforcement provided by the present invention comprises carbon fiber and linear phenolic fiber; the raw materials for preparing the linear phenolic fiber comprise a toughening system, boric acid and a first linear phenolic resin in a mass ratio of (10-30):(0.8-1):(69.2-89) in sequence. Under the above ratio, the toughening system can be quickly melted with the first linear phenolic resin and the boric acid to form a homogeneous body. Boric acid mainly plays the role of a modifier, and can specifically be used as a carbonizing agent in the subsequent combustion process, so that the phenolic-epoxy curing system is transformed from decomposing small molecular hydrocarbons to forming a dehydrated carbon layer during the flame retardant process. The functional fiber reinforcement can overcome the shortcomings of woven fabric reinforcement and warp knitted fabric reinforcement, and solve the dilemma that unidirectional tows cannot be effectively introduced in vacuum.

[0047] By introducing linear phenolic fiber with flame retardant properties into the carbon fiber fabric system in the form of a woven fabric, the linear phenolic fiber can be used as a curing agent for epoxy resin to participate in the reaction after melting in the melting section (95°C to 120°C), and dissolve in the epoxy resin matrix during the reaction. The fiber form automatically changes from the original different woven fabrics to the unidirectional tape form, and the fiber organization form is changed during the curing process. At the same time, the linear phenolic resin and anhydride curing agent already in the vacuum-introduced resin system are used as curing agents for epoxy resin to participate in the high-temperature curing reaction, which indirectly improves the flame retardant properties of the entire product, thereby achieving structural flame retardancy. The above method improves the flame retardant properties of the overall product while realizing the ingenious transformation and use of the unidirectional tape reinforcement in vacuum introduction.

[0048] The functional fiber reinforcement provided by the present invention can be effectively combined with the flame retardant resin system for vacuum introduction to achieve structural flame retardancy, improve the "charring" characteristics during the combustion process, and thus achieve the highest flame retardancy level HL3 of R1 in EN45545-2 without affecting the back-end introduction process. In addition, by introducing the above-mentioned functional fiber reinforcement, the shortcomings of woven fabric reinforcement and warp knitted fabric reinforcement can be cleverly overcome, and the dilemma that unidirectional tow cannot be effectively introduced in vacuum can be solved. The preparation method of the corresponding composite material is simple, easy to operate, and can be industrialized. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0050] Figure 1 This is a schematic diagram of a 2 / 2 twill weave;

[0051] Figure 2 This is a schematic diagram of the weaving of twill 3 / 1 form;

[0052] Figure 3 It is the structural diagram of the vacuum system;

[0053] Figure 4 Schematic diagram of the vacuum infusion curing process. DETAILED DESCRIPTION

[0054] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0055] The functional fiber reinforcement, composite material and preparation method thereof provided by the present invention are described in detail below.

[0056] The present invention provides a functional fiber reinforcement, which comprises carbon fiber and linear phenolic fiber.

[0057] The raw materials for preparing the linear phenolic fiber include a toughening system, boric acid and a first linear phenolic resin in a mass ratio of (10-30):(0.8-1):(69.2-89).

[0058] The linear phenolic fiber is prepared by melt extrusion spinning of a toughening system, boric acid and a first linear phenolic resin according to the above proportions.

[0059] In some optional embodiments, the mass ratio of the toughening system, boric acid and the first linear phenolic resin can be (15-20):(0.8-0.9):(79.2-84.1), such as 15:0.9:84.1 or 20:0.8:79.2.

[0060] The toughening system may exemplarily include at least one of nylon series block, polypropylene, polyethersulfone and polyaryletherketone. The above substances have better toughening performance.

[0061] Particle size D of toughening system 90 ≤90μm, such as 90μm, 80μm, 70μm, 60μm, 50μm, 40μm, 30μm, 20μm or 10μm, etc., and can also be other values ​​within the range of ≤90μm.

[0062] The use of the toughening system within the above particle size range is beneficial to increasing the heating area during the melting process, reducing the time of melt extrusion, and can quickly melt with the first linear phenolic formaldehyde and boric acid to form a uniform body.

[0063] The boric acid mentioned above mainly plays the role of a modifier, specifically as a carbonizing agent in the subsequent combustion process, and in the process of flame retardancy, the phenolic-epoxy curing system is transformed from the decomposition of small molecular hydrocarbon-containing combustion to the formation of a dehydrated carbon layer.

[0064] The melting point of the first linear phenolic resin may be 95°C to 120°C, such as 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, or other values ​​within the range of 95°C to 120°C.

[0065] If the melting point of the first linear phenolic resin is lower than 95, it is not conducive to the subsequent melt extrusion spinning, the spinning strength is insufficient, and the subsequent functional fiber weaving is affected; if the melting point of the first linear phenolic resin is higher than 120, it is not conducive to the early melt extrusion process, the melt extrusion rate is low, and the wire breakage and mold blocking are prone to occur.

[0066] In the above, the first linear phenolic resin having the above melting point and number average molecular weight can be melt extruded and spun with the toughening system better. In addition, the first linear phenolic resin also has better combustion charring performance.

[0067] Exemplarily, the diameter of the linear phenolic fiber may be 12 μm to 14 μm, such as 12 μm, 12.5 μm, 13 μm, 13.5 μm or 14 μm, etc., or may be other values ​​within the range of 12 μm to 14 μm.

[0068] In the present invention, the functional fiber reinforcement is obtained by mixing carbon fibers and linear phenolic fibers.

[0069] The carbon fiber may be exemplarily T700 grade carbon fiber produced by Jiangsu Hengshen Co., Ltd.

[0070] In some embodiments, the functional fiber reinforcement includes warp direction fibers and weft direction fibers, wherein the warp direction fibers are carbon fiber bundles and the weft direction fibers are linear phenolic fibers.

[0071] Different forms of woven fabrics can be obtained by adopting different mixed forms. Exemplarily, the mixed weaving forms may include plain 1 / 1 form, twill 2 / 2 form, twill 3 / 1 form, satin 5S form or satin 8S form, etc. In use, for the same yarn bundle woven fabric in different directions, the above weaving methods have better deformability in turn, that is, plain 1 / 1 form < twill 2 / 2 form < twill 3 / 1 form < satin 5S form < satin 8S form, but it also means that the weight ratio of the first linear phenolic resin per unit area decreases in turn, which will reduce the flame retardant properties of the subsequent overall component structure. Comprehensively weighing, in some typical embodiments, the weaving form is a twill 2 / 2 form (such as Figure 1 as shown) or twill 3 / 1 form (as Figure 2 shown), Figure 1 and Figure 2 The medium black is linear phenolic fiber and the gray is carbon fiber.

[0072] In some optional embodiments, the total number of carbon fiber tows in the functional fiber reinforcement can be 3,000 to 50,000, such as 3,000, 6,000, 12,000, 24,000 or 50,000, or other values ​​within the range of 3,000 to 50,000.

[0073] The total amount of the linear phenolic fiber tows may be 1500 to 6000, such as 1500, 3000 or 6000, or other values ​​within the range of 1500 to 6000.

[0074] As mentioned above, the functional fiber reinforcement provided by the present invention can be effectively combined with the flame retardant resin system for vacuum introduction to achieve structural flame retardancy, improve the "charring" characteristics during the combustion process, and thus achieve the highest flame retardancy level HL3 of R1 in EN45545-2 without affecting the back-end introduction process. In addition, by introducing the above-mentioned functional fiber reinforcement, the shortcomings of woven fabric reinforcement and warp knitted fabric reinforcement can be cleverly overcome, solving the dilemma that unidirectional tow cannot be effectively introduced in vacuum.

[0075] Correspondingly, the present invention also provides a composite material, the raw materials for preparing the composite material include a flame retardant resin system for vacuum introduction and the above-mentioned functional fiber reinforcement.

[0076] In some optional embodiments, the mass ratio of the flame retardant resin system for vacuum introduction to the functional fiber reinforcement can be 3.5:6.5 to 4.5:5.5, such as 3.5:6.5, 4:6 or 4.5:5.5, or other values ​​within the range of 4:6 to 4.5:5.5.

[0077] In the present invention, the flame retardant resin system for vacuum introduction comprises an epoxy resin component, a flame retardant resin component, a toughening resin component and a curing agent component.

[0078] In some optional embodiments, the mass ratio of the epoxy resin component, the flame retardant resin component, the toughening resin component and the curing agent component can be (49-51):(14-18):10:(23-25), such as 49:18:10:23, 50:16:10:24 or 51:14:10:25, etc., or it can be other values ​​within the range of (49-51):(14-18):10:(23-25).

[0079] In some optional embodiments, the viscosity of the flame retardant resin system for vacuum introduction at 25° C. may be 400 cps to 1200 cps, such as 400 cps, 600 cps, 800 cps, 1000 cps or 1200 cps, or other values ​​within the range of 400 cps to 1200 cps.

[0080] In some optional embodiments, the epoxy resin component includes epoxy resin and may further include an epoxy reactive diluent.

[0081] The epoxy resin may include at least one of bisphenol A epoxy resin and bisphenol F epoxy resin. Wherein, the bisphenol A epoxy resin may include at least one of E-51 liquid resin, E-54 liquid resin, E-44 liquid resin and NPEL127 liquid resin. The bisphenol F epoxy resin may include NPEF-170 epoxy resin. The epoxy reactive diluent may include at least one of XY622, XY699 and XY678.

[0082] In some alternative embodiments, the flame retardant resin component may include at least one of a second phenolic novolac resin and a phosphorus-containing epoxy resin.

[0083] The melting point of the second linear phenolic resin may be 60°C to 80°C, such as 60°C, 65°C, 70, 75°C or 80°C, or other values ​​within the range of 60°C to 80°C.

[0084] The phosphorus-containing epoxy resin may include at least one of a phosphorus-containing epoxy resin modified by phosphate esters and a phosphorus-containing epoxy resin modified by DOPO. The phosphorus-containing epoxy resin modified by phosphate esters may include at least one of FR-633 and FR-7016. The phosphorus-containing epoxy resin modified by DOPO may include at least one of D200, D201 and D202.

[0085] In some optional embodiments, the toughening resin component may include at least one of a polyurethane-modified epoxy resin, a carboxyl-terminated nitrile rubber resin, a dimer acid-modified epoxy resin, and a core-shell particle toughening resin containing nano rubber particles.

[0086] The polyurethane-modified epoxy resin may include EPU133.

[0087] The carboxyl-terminated nitrile rubber resin may include at least one of CTBN1300X13, CTBN1300X8 and CTBN1300X31.

[0088] The dimer acid-modified epoxy resin may include at least one of HyPox DA323 and YD-172.

[0089] The core-shell particle toughening resin containing nano rubber particles may include at least one of MX-962, MX-150 and MX-160.

[0090] In some optional embodiments, the curing agent component includes at least one of a liquid acid anhydride curing agent and a modified liquid acid anhydride curing agent, and may further include a liquid accelerator.

[0091] The modified liquid anhydride curing agent may include YEG-1070.

[0092] The liquid accelerator may include at least one of an imidazole-modified liquid accelerator and a complex-type liquid modifier. The imidazole-modified liquid accelerator may include at least one of 2E4MZ-CN and 2PHZ-CN. The complex-type liquid modifier may include at least one of Anchor 1170, Anchor 1171, Anchor 1053, and Anchor 1115.

[0093] In addition, the present invention also provides a method for preparing the above-mentioned composite material, comprising the following steps: vacuum-introducing a preform made of functional fiber reinforcement and a flame-retardant resin system for vacuum introduction, keeping warm at 95°C to 120°C for 1h to 3h, and then curing at 130°C to 150°C.

[0094] In some optional embodiments, the preparation of the preform may include: laying the functional fiber reinforcement in a preset laying direction, and maintaining the preform under negative pressure at 90° C. to 100° C. for 20 min to 30 min.

[0095] The laying direction can be changed according to different applications. For example, it can be laid at 0°, or laid alternately at 0° and 90°, or laid alternately at 0°, -45°, 45° and 90°.

[0096] The negative pressure holding temperature may be 90° C., 95° C., or 100° C., or other values ​​within the range of 90° C. to 100° C. The negative pressure holding time may be 20 min., 25 min., or 30 min., or other values ​​within the range of 20 min to 30 min.

[0097] After the flame retardant resin system for vacuum introduction is introduced, the insulation temperature may be 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, etc., or other values ​​within the range of 95°C to 120°C.

[0098] After the flame retardant resin system for vacuum introduction is introduced, the heat preservation time can be 1h, 1.5h, 2h, 2.5h or 3h, etc., and can also be other values ​​within the range of 1h to 3h.

[0099] Through the above-mentioned heat preservation process, the linear phenolic fiber in the functional fiber reinforcement is fully melted into the flame-retardant resin system for vacuum introduction to participate in the curing reaction.

[0100] The curing temperature may be 130°C, 135°C, 140°C, 145°C or 150°C, etc., or other values ​​within the range of 130°C to 150°C.

[0101] The vacuum system used in the present invention includes a vacuum valve group, a demoulding cloth, a baffle, a laminate, a mold, a sealing tape, a vacuum bag, a one-way air permeable film (VAP film) and a guide net. The specific location and working principle of each structure can refer to the relevant prior art (such as Figure 3 The main process of vacuum introduction curing can also refer to the prior art. The schematic diagram of vacuum introduction curing corresponding to the present invention is as follows Figure 4 As shown, no further elaboration is given here.

[0102] The inventors need to emphasize that if the vacuum-introduced liquid resin meets EN45545-2, only through the flame retardant modification of epoxy resin, such as grafting modification, there will be the following problems: First, the cost of a single grafted modified epoxy resin is high, and the amount added to the resin system needs to account for more than 60%. Second, it is difficult for a single grafted modified epoxy resin to achieve the requirements of EN45545-2 for critical flame intensity and average maximum heat release.

[0103] In addition, the vacuum introduction process has certain requirements for fiber reinforcement, especially carbon fiber as a vacuum introduction reinforcement material. There are three main forms of carbon fiber reinforcement: pure unidirectional method (applicable to prepreg manufacturing method), fabric method and warp knitting method. The above three methods require pre-forming treatment for complex parts before application. For the pure unidirectional method, it is basically impossible to achieve completion. The reason is that the pure unidirectional laying method cannot be bound in the 90° direction, and the shaping force is difficult to be stronger than the subsequent resin introduction flushing force, which ultimately leads to the fiber being inconsistent with the design, and ultimately leads to unstable product performance. For the fabric method, although there is no problem of unidirectional laying, due to the relatively wide and thick interweaving points of the fabric, the carbon fiber bundles used for weaving are mostly composed of 3,000 or 12,000 7μm carbon fiber filaments, which have certain defects in the penetration of the resin at the interweaving points. The final product will have certain defects in appearance, and it is necessary to complete the appearance requirements of the product through post-repair (such as glue filling). For the warp knitted fabric method, although it can overcome the pressure scouring and curing flow scouring of pure unidirectional covering and subsequent resin introduction, and the shape of the fiber is fixed by the longitudinal paving method, the fibers at the paving are bundled, which will affect the performance of the fiber reinforcement later. At the same time, due to the large gram weight of the warp knitted fabric (the corresponding thickness is also thick), it is not conducive to the introduction of vacuum resin, and it is easy to have post-process technical problems such as uneven surface of the part due to insufficient infiltration.

[0104] The present invention starts from the source, introduces linear phenolic fiber with flame retardant performance into the carbon fiber fabric system in the form of a woven fabric, and after the linear phenolic fiber is melted in the melting section (95°C to 120°C), it can participate in the reaction as a curing agent for epoxy resin, and dissolves in the epoxy resin matrix during the reaction, and the fiber form automatically changes from the original different woven fabrics to the unidirectional tape form, and changes the organizational form of the fiber during the curing process. At the same time, the linear phenolic resin and acid anhydride curing agent that are already present in the vacuum introduction resin system participate in the high-temperature curing reaction as a curing agent for epoxy resin, indirectly improving the flame retardant performance of the entire product, and then achieving structural flame retardancy. The above method improves the flame retardant performance of the overall product while realizing the ingenious transformation and use of the unidirectional tape reinforcement in vacuum introduction.

[0105] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0106] Example 1

[0107] This embodiment provides a composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product A1"), and the preparation method thereof includes:

[0108] S1: Preparing a preform of a functional fiber reinforcement.

[0109] S11: preparing a linear phenolic fiber bundle: mixing a nylon 6 / 66 / 12 terpolymer, boric acid and a first linear phenolic resin in a mass ratio of 15:0.9:84.1, and then performing melt extrusion spinning to prepare a desired linear phenolic fiber bundle.

[0110] Among them, the particle size D of nylon 6 / 66 / 12 terpolymer 90 The melting point of the first linear phenolic resin is 105° C. The first linear phenolic resin is specifically a linear phenolic resin of model WL-8219 produced by Weilin Technology Co., Ltd. The diameter of the fiber in the linear phenolic fiber bundle is 13 μm.

[0111] S12: Prepare carbon fiber: use T700 grade carbon fiber from Hengshen Co., Ltd.

[0112] S13: Preparation of functional fiber reinforcement: Using carbon fiber bundles as warp fibers and linear phenolic fibers as weft fibers, the carbon fibers and linear phenolic fibers are mixed in a 2 / 2 twill weave to obtain a functional fiber reinforcement.

[0113] The total amount of linear phenolic fiber bundles in the functional fiber reinforcement is 1500, and the total amount of carbon fiber bundles is 3000.

[0114] S14: Laying and shaping: Laying the functional fiber reinforcement alternately in the 0° and 90° directions, and maintaining the preform under negative pressure for 20 minutes at 90°C to complete the shaping of the preform.

[0115] S2: Preparation of flame retardant resin system for vacuum introduction.

[0116] The raw materials for preparing the flame-retardant resin system for vacuum introduction include 51 parts of conventional epoxy resin components, 14 parts of flame-retardant resin components, 10 parts of toughening resin components and 25 parts of curing agent components in terms of mass.

[0117] Specifically, 30 parts of bisphenol A epoxy resin, 20 parts of bisphenol F epoxy resin and 1 part of epoxy active diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is fully stirred until it is evenly mixed; 14 parts of a second linear phenolic resin are added, and the mixture is fully stirred until it is evenly mixed; 10 parts of a core-shell epoxy toughening resin are added, and the mixture is fully stirred, and the temperature is lowered to 30°C; 11.5 parts of a phosphorus-modified anhydride curing agent, 13 parts of methyltetrahydrophthalic anhydride and 0.5 parts of an imidazole-modified liquid accelerator are added, and the mixture is evenly stirred for 15 minutes to obtain the flame-retardant resin system a1 for vacuum introduction (the viscosity at 25°C is 450 cps), and the resin system needs to be used within 24 hours.

[0118] Among them, bisphenol A epoxy resin is a product of model NPEL127 produced by Kunshan Nan Ya Company; bisphenol F epoxy resin is a product of model NPEF170 produced by Kunshan Nan Ya Company; epoxy reactive diluent is a product of model XY622 produced by Xinyuan Technology Company; the second linear phenolic resin is a product of model WL-8315 produced by Weilin Co., Ltd.; core-shell epoxy toughening resin is a product of model MX-962 produced by Zhongyuan Chemical Company; phosphorus-modified anhydride curing agent is a product of model YEG-1070 produced by Guangdong Guangshan Company; imidazole-modified liquid accelerator is a product of model 2E4MZ-CN produced by Shikoku Chemical Company.

[0119] S4: preparing a composite material.

[0120] The flame-retardant resin system a1 for vacuum introduction and the preform of the functional fiber reinforcement laid in advance are vacuum introduced (the mass ratio of the flame-retardant resin system for vacuum introduction to the functional fiber reinforcement is 4:6), and after being kept at 100°C in a vacuum system for 2 hours, the temperature is raised to 130°C for high-temperature curing to complete the overall curing of the resin system, thereby obtaining the product A1.

[0121] Example 2

[0122] The difference between this embodiment and embodiment 1 is that the flame retardant resin system for vacuum introduction in S2 has 14 parts of phosphorus-containing epoxy resin as the flame retardant resin component and 10 parts of polyurethane-modified toughening resin as the toughening resin component. The flame retardant resin system for vacuum introduction is denoted as b1 (viscosity at 25° C. is 580 cps).

[0123] Among them, the phosphorus-containing epoxy resin is a product of model D200 produced by Amonte Company; the polyurethane modified toughening resin is a product of model EPU133 produced by Complex Chemical Company.

[0124] The manufactured product obtained in this embodiment is denoted as B1.

[0125] Example 3

[0126] The difference between this embodiment and embodiment 1 is that:

[0127] In S11, the mass ratio of the nylon 6 / 66 / 12 terpolymer, boric acid, and the first linear phenolic resin is 20:0.8:79.2.

[0128] In S13, the mixed weaving is carried out in the form of twill 3 / 1.

[0129] In S2, the raw materials for preparing the flame retardant resin system for vacuum introduction include 49 parts of conventional epoxy resin components, 18 parts of flame retardant resin components, 10 parts of toughening resin components and 23 parts of curing agent components.

[0130] Specifically, 30 parts of bisphenol A epoxy resin, 15 parts of bisphenol F epoxy resin and 4 parts of epoxy active diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is fully stirred until it is evenly mixed; 18 parts of a second linear phenolic resin are added, and the mixture is fully stirred until it is evenly mixed; 10 parts of a core-shell epoxy toughening resin are added, and the mixture is fully stirred, and the temperature is lowered to 30°C, 10.5 parts of a phosphorus-modified anhydride curing agent, 12 parts of methyltetrahydrophthalic anhydride and 0.5 parts of an imidazole-modified liquid accelerator are added, and the mixture is evenly stirred for 15 minutes to obtain the vacuum-introduced resin system c1 (viscosity at 25°C is 670 cps), and the resin system needs to be used within 24 hours.

[0131] The manufactured product obtained in this embodiment is denoted as C1.

[0132] Example 4

[0133] The difference between this embodiment and embodiment 1 is that:

[0134] In S11, the mass ratio of the nylon 6 / 66 / 12 terpolymer, boric acid, and the first linear phenolic resin is 20:0.8:79.2.

[0135] In S2, the raw materials for preparing the flame retardant resin system for vacuum introduction include 51 parts of conventional epoxy resin components, 14 parts of flame retardant resin components, 10 parts of toughening resin components and 20 parts of curing agent components.

[0136] Specifically, 30 parts of bisphenol A epoxy resin, 20 parts of bisphenol F epoxy resin and 1 part of epoxy reactive diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is stirred thoroughly until uniformly mixed; 8 parts of a second linear phenolic resin and 6 parts of a phosphorus-containing epoxy resin (the material is the same as in Example 2) are added, and the mixture is stirred thoroughly until uniformly mixed; 10 parts of a polyurethane-modified toughening resin (the material is the same as in Example 2) are added, and the mixture is stirred thoroughly, and the temperature is lowered to 30°C; 11.5 parts of a phosphorus-modified anhydride curing agent, 13 parts of methyltetrahydrophthalic anhydride and 0.5 parts of an imidazole-modified liquid accelerator are added, and the mixture is stirred uniformly for 15 minutes to obtain the vacuum-introduced resin system d1 (viscosity at 25°C is 620 cps), and the resin system needs to be used within 24 hours.

[0137] The manufactured product obtained in this embodiment is denoted as D1.

[0138] Example 5

[0139] This embodiment provides a composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product E1"), and the preparation method thereof includes:

[0140] S1: Preparing a preform of a functional fiber reinforcement.

[0141] S11: preparing a linear phenolic fiber bundle: mixing nylon 6 / 66 / 1010, polyethersulfone, boric acid and a first linear phenolic resin in a mass ratio of 14:1:0.9:84.1, and then performing melt extrusion spinning to prepare a desired linear phenolic fiber bundle.

[0142] Among them, the particle size D of nylon 6 / 66 / 1010 90 80μm; the particle size of polyethersulfone D 95 The melting point of the first linear phenolic resin is 120° C. The first linear phenolic resin is specifically a linear phenolic resin of model WL-8308 produced by Weilin Co., Ltd. The diameter of the fiber in the linear phenolic fiber bundle is 14 μm.

[0143] S12: Prepare carbon fiber: The carbon fiber bundle uses T700 grade carbon fiber produced by Hengshen Co., Ltd.

[0144] S13: Preparation of functional fiber reinforcement: Using carbon fiber bundles as warp fibers and linear phenolic fibers as weft fibers, the carbon fibers and linear phenolic fibers are mixed in a plain 1 / 1 weaving form to obtain a functional fiber reinforcement.

[0145] The total amount of linear phenolic fiber bundles in the functional fiber reinforcement is 3000, and the total amount of carbon fiber bundles is 6000.

[0146] S14: Laying and shaping: Laying the functional fiber reinforcement alternately in the 0° and 90° directions, and maintaining the preform under negative pressure for 20 minutes at 90°C to complete the shaping of the preform.

[0147] S2: Preparation of flame retardant resin system for vacuum introduction.

[0148] Calculated by weight, the raw materials for preparing the flame-retardant resin system for vacuum introduction include 49 parts of conventional epoxy resin components, 18 parts of flame-retardant resin components, 10 parts of toughening resin components and 23 parts of curing agent components.

[0149] Specifically, 30 parts of bisphenol A epoxy resin, 19 parts of bisphenol F epoxy resin and 1 part of epoxy active diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is stirred thoroughly until it is evenly mixed; 18 parts of a second linear phenolic resin are added, and the mixture is stirred thoroughly until it is evenly mixed; 10 parts of a carboxyl-terminated nitrile rubber resin are added, and the mixture is stirred thoroughly, and the temperature is lowered to 30°C; 9.5 parts of a phosphorus-modified anhydride curing agent, 13 parts of methyltetrahydrophthalic anhydride and 0.5 parts of an imidazole-modified liquid accelerator are added, and the mixture is stirred evenly for 15 minutes to obtain the flame-retardant resin system e1 for vacuum introduction (the viscosity at 25°C is 770 cps), and the resin system needs to be used within 24 hours.

[0150] The carboxyl-terminated nitrile rubber resin is a product of model CTBN1300X13 produced by Huntsman, and the sources of other raw materials are the same as those in Example 1.

[0151] S4: preparing a composite material.

[0152] The flame-retardant resin system e1 for vacuum introduction and the preform of the functional fiber reinforcement laid in advance are vacuum introduced (the mass ratio of the flame-retardant resin system for vacuum introduction to the functional fiber reinforcement is 4:6), and after being kept at 95°C in a vacuum system for 3 hours, the temperature is raised to 130°C for high-temperature curing to complete the overall curing of the resin system, thereby obtaining the product E1.

[0153] Example 6

[0154] This embodiment provides a composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product F1"), and the preparation method thereof includes:

[0155] S1: Preparing a preform of a functional fiber reinforcement.

[0156] S11: preparing a linear phenolic fiber bundle: mixing nylon 6 / 66 / 1010, polyaryletherketone, boric acid and a first linear phenolic resin in a mass ratio of 19:1:0.8:79.2, and then performing melt extrusion spinning to prepare a desired linear phenolic fiber bundle.

[0157] Among them, the particle size D of nylon 6 / 66 / 1010 90 80 μm; the particle size D of polyaryletherketone 95 The melting point of the first linear phenolic resin is 110° C. The first linear phenolic resin is specifically a linear phenolic resin of model WL-8206 produced by Weilin Co., Ltd. The diameter of the fiber in the linear phenolic fiber bundle is 13 μm.

[0158] S12: Prepare carbon fiber: The carbon fiber bundle uses T700 grade carbon fiber produced by Hengshen Co., Ltd.

[0159] S13: Preparation of functional fiber reinforcement: Using carbon fiber bundles as warp fibers and linear phenolic fibers as weft fibers, the carbon fibers and linear phenolic fibers are mixed in a satin 5S weaving form to obtain a functional fiber reinforcement.

[0160] The total amount of linear phenolic fiber bundles in the functional fiber reinforcement is 6000, and the total amount of carbon fiber bundles is 12000.

[0161] S14: Laying and shaping: Laying the functional fiber reinforcement alternately in the 0° and 90° directions, and maintaining the preform under negative pressure for 20 minutes at 90°C to complete the shaping of the preform.

[0162] S2: Preparation of flame retardant resin system for vacuum introduction.

[0163] The raw materials for preparing the flame-retardant resin system for vacuum introduction include 51 parts of conventional epoxy resin components, 14 parts of flame-retardant resin components, 10 parts of toughening resin components and 25 parts of curing agent components in terms of mass.

[0164] Specifically, 30 parts of bisphenol A epoxy resin, 21 parts of bisphenol F epoxy resin and 1 part of epoxy active diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is fully stirred until it is evenly mixed; 14 parts of a second linear phenolic resin are added, and the mixture is fully stirred until it is evenly mixed; 10 parts of a dimer acid-modified epoxy resin are added, and the mixture is fully stirred, and the temperature is lowered to 30°C; 11.5 parts of a phosphorus-modified anhydride curing agent, 13 parts of methyltetrahydrophthalic anhydride and 0.5 parts of a complex-type liquid modifier are added, and the mixture is evenly stirred for 15 minutes to obtain the flame-retardant resin system f1 for vacuum introduction (the viscosity at 25°C is 890cps), and the resin system needs to be used within 24 hours.

[0165] The epoxy resin modified by dimer acid is a product of model number HyPox DA323 produced by Jiadida Company, and the sources of other raw materials are the same as those in Example 1.

[0166] S4: preparing a composite material.

[0167] The flame-retardant resin system f1 for vacuum introduction and the preform of the functional fiber reinforcement laid in advance are vacuum introduced (the mass ratio of the flame-retardant resin system for vacuum introduction to the functional fiber reinforcement is 5:5), and after being kept at 120°C in a vacuum system for 1 hour, the temperature is raised to 130°C for high-temperature curing to complete the overall curing of the resin system, thereby obtaining the product F1.

[0168] Comparative Example 1

[0169] This comparative example provides a conventional composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product G1"), and its preparation method includes:

[0170] S1: Prepare a twill 2 / 2 carbon fiber woven fabric, wherein the carbon fiber is the same as that in Example 1.

[0171] S2: Preparation of flame retardant resin system for vacuum introduction.

[0172] The raw materials for preparing the flame-retardant resin system for vacuum introduction include 16 parts of conventional epoxy resin components, 18 parts of flame-retardant resin components, 6 parts of toughening resin components, 20 parts of flame retardant components and 40 parts of curing agent components in parts by mass.

[0173] Specifically, 7 parts of bisphenol A epoxy resin, 6 parts of bisphenol F epoxy resin and 3 parts of epoxy active diluent are added to a mixing kettle, the temperature is raised to 85°C, and the mixture is fully stirred until it is evenly mixed; 18 parts of linear phenolic resin are added, and the mixture is fully stirred until it is evenly mixed; 6 parts of polyurethane modified toughening resin are added, and the mixture is fully stirred, and then 17 parts of flame retardant ammonium polyphosphate and 3 parts of zinc borate are added, and the mixture is stirred evenly, and the temperature is lowered to 30°C; 14.5 parts of phosphorus-modified anhydride curing agent, 25 parts of methyltetrahydrophthalic anhydride and 0.5 parts of imidazole-modified liquid accelerator are added, and the mixture is evenly stirred for 15 minutes to obtain the vacuum-introduced resin system e1, which needs to be used within 24 hours.

[0174] The sources of the raw materials used in this step refer to Example 1 and Example 2.

[0175] S3: preparing a composite material.

[0176] The vacuum-introduced resin system e1 was vacuum-introduced into the twill 2 / 2 carbon fiber woven fabric (the mass ratio of the flame-retardant resin system for vacuum introducing to the functional fiber reinforcement was 4:6), and after being kept at 100°C for 2 hours in a vacuum system, the temperature was raised to 130°C for high-temperature curing to complete the overall curing of the resin system, thereby obtaining the manufactured product G1.

[0177] Comparative Example 2

[0178] This comparative example provides a conventional composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product H1"), and its preparation method includes:

[0179] S1: Prepare a 0 / 90 biaxial warp knitted fabric, the carbon fibers of which are the same as those of Example 1.

[0180] S2: Prepare a flame retardant resin system for vacuum introduction, the same as Comparative Example 1.

[0181] S3: preparing a composite material.

[0182] The vacuum-introduced resin system e1 and the 0 / 90 biaxial warp knitted fabric were vacuum-introduced (the mass ratio of the flame-retardant resin system for vacuum introducing to the functional fiber reinforcement was 4:6), and after being kept at 100°C for 2 hours, the temperature was raised to 130°C for high-temperature post-curing to complete the overall curing of the resin system, thereby obtaining the manufactured product H1.

[0183] Comparative Example 3

[0184] This comparative example provides a conventional composite material that meets the flame retardant requirements of EN45545-2 (hereinafter referred to as "product I1"), and its preparation method includes:

[0185] S1: Same as Comparative Example 1.

[0186] S2: preparing a flame retardant resin system for vacuum introduction, the same as in Example 1.

[0187] S3: Same as Comparative Example 1.

[0188] The manufactured product obtained in this comparative example is recorded as I1.

[0189] Test example

[0190] The laminate-level performance tests were conducted on the manufactured products obtained in the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 3, and the results are shown in Tables 1 to 3.

[0191] Among them, the test standards for warp tensile strength and weft tensile strength refer to ASTM D3039, the test standards for warp compressive strength and weft compressive strength refer to ASTM D6641, the test standard for interlaminar shear strength refers to ASTM D2344, the test standard for laminate porosity refers to GB / T 3365, and the test standard for flame retardant performance refers to EN45545-2. The detailed requirements for each level of EN45545-2 standard are shown in Table 3.

[0192] Table 1 Laminate-level properties of different embodiments

[0193] Test items Test Standards A1 B1 C1 D1 E1 F1 G1 H1 I1 Warp tensile strength / Mpa ASTM D3039 967 893 1105 903 831 897 593 665 699 Weft tensile strength / Mpa ASTM D3039 72.7 71.3 75.6 72.1 70.5 71.1 68.5 69.1 69.6 Warp compression strength / Mpa ASTM D6641 832 783 896 817 757 785 554 606 615 Weft compression strength / Mpa ASTM D6641 71.3 69.6 72.1 70.5 65.6 67.3 65.3 66.8 68.3 Interlaminar shear strength / Mpa ASTM D2344 64.3 62.7 67.2 63.7 58.4 59.6 51.9 53.3 63.5 Laminate porosity / % GB / T 3365 0.63 0.75 0.65 0.81 0.92 0.87 5.7 3.9 0.77

[0194] Table 2 Flame retardant properties of laminates in different embodiments and comparative examples

[0195] Test Standards <![CDATA[CEF / kW / m 2 ]]> <![CDATA[MARHE / kW / m 2 ]]> Ds(4) <![CDATA[VOF4]]> <![CDATA[CIT G ]]> Flame retardant grade A1 EN45545-2 50 27 12 15 0.16 HL3 B1 EN45545-2 39 53 106 197 0.22 HL3 C1 EN45545-2 50 29 25 39 0.18 HL3 D1 EN45545-2 45 42 57 89 0.20 HL3 E1 EN45545-2 50 25 12 13 0.17 HL3 F1 EN45545-2 41 48 69 107 0.18 HL3 G1 EN45545-2 28 82 179 387 0.19 HL2 H1 EN45545-2 32 78 161 332 0.21 HL2 I1 EN45545-2 40 58 151 302 0.18 HL2

[0196] Table 3 EN45545-2 standard requirements for each level

[0197] Test items Test Method Parameter / Unit HL1 HL2 HL3 Critical radiation energy ISO5658-2 <![CDATA[CFE / KW / m 2 ]]> ≥20 ≥20 ≥20 Heat release <![CDATA[ISO5660-1(50KW / m 2 )]]> <![CDATA[MARHE / KW / m 2 ]]> -- ≤90 ≤60 Smoke density <![CDATA[EN ISO5659-2(50KW / m 2 )]]> Ds(4) / Dimension ≤600 ≤300 ≤150 Smoke density <![CDATA[EN ISO5659-2(50KW / m 2 )]]> VOF(4) / min ≤1200 ≤600 ≤300 Toxicity of smoke <![CDATA[EN ISO5659-2(50KW / m 2 )]]> CIT / dimension ≤1.20 ≤0.90 ≤0.75

[0198] From the mechanical properties and flame retardant properties of the embodiments (A1~F1) and the comparative examples (G1~Q1), it can be seen that the plate-level performance and flame retardant properties of the parts using the new vacuum introduction process design method are significantly better than those of the comparative examples. The main reason is that the functional fiber reinforcement cleverly used in the embodiments of the present invention gradually dissolves into the vacuum introduction resin as the temperature rises during the later resin curing process, and participates in the curing reaction as a curing agent for the epoxy resin; for the vacuum introduction resin, the introduction of flame retardant resin and flame retardant powder can be minimized, so that the vacuum introduction resin has more excellent introduction process characteristics, and the later plate porosity and mechanical properties are relatively excellent. During the entire curing process, the linear phenolic fiber bundles in the functional fiber reinforcement dissolve into the resin system, and the layout structure of the fibers is changed, from the original 2 / 2 or 3 / 1 fabric form to the unidirectional tape form, reducing the bending deformation point in the warp direction of the fibers, which is also an important reason why the warp tensile properties in the embodiments are generally higher.

[0199] Comparative Examples G1 and H1 introduced a traditional flame retardant resin system. During the vacuum introduction process, serious sedimentation problems occurred between fiber layers and uneven introduction flow problems occurred, which resulted in a significant decrease in the mechanical properties of the corresponding laminates compared to the examples. At the same time, the porosity data also indirectly reflected the poor performance of the comparative example boards.

[0200] From Table 2, the flame retardant performance of the embodiment of the present invention can be effectively improved compared with the comparative example. The cleverness lies in the introduction of flame retardant fibers into the fabric, and the flame retardant fibers can be integrated into the overall resin system during the curing process and participate in the curing reaction, effectively achieving structural flame retardancy. Thus, the HL3 flame retardant grade is achieved under the flame retardant requirements of EN45545-2 (critical radiation energy, heat release, smoke density, smoke concentration, and smoke toxicity meet the requirements at the same time).

[0201] In summary, the present invention achieves structural flame retardancy by effectively combining functional fiber reinforcement with a flame retardant resin system for vacuum introduction, improves the "charring" characteristics during the combustion process, and thus achieves the highest flame retardancy level HL3 of R1 in EN45545-2 without affecting the back-end introduction process. In addition, by introducing functional fiber reinforcement, the shortcomings of woven fabric reinforcement and warp knitted fabric reinforcement are cleverly overcome, and the dilemma that unidirectional tows cannot be effectively introduced in vacuum is solved. The preparation method of the corresponding composite material is simple, easy to operate, and can be industrialized.

[0202] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A functional fiber reinforcement, characterized in that: The functional fiber reinforcement comprises carbon fiber and linear phenolic fiber, and the functional fiber reinforcement is obtained by mixing the carbon fiber and the linear phenolic fiber; Among them, the raw materials for preparing linear phenolic fiber include a toughening system, boric acid and a first linear phenolic resin in a mass ratio of (10-30):(0.8-1):(69.2-89); the toughening system includes at least one of nylon block copolymer, polypropylene, polyether sulfone and polyaryletherketone.

2. The functional fiber reinforcement according to claim 1, characterized in that: The linear phenolic fiber has at least one of the following characteristics: Feature 1: Particle size D of the toughening system 90 ≤90μm; Feature 2: The melting point of the first linear phenolic resin is 95°C to 120°C; Feature 3: The diameter of the linear phenolic fiber is 12 μm to 14 μm.

3. The functional fiber reinforcement according to claim 1 or 2, characterized in that: The functional fiber reinforcement comprises warp direction fibers and weft direction fibers, wherein the warp direction fibers are carbon fiber bundles, and the weft direction fibers are the linear phenolic fibers; Preferably, the mixed weaving form includes a plain 1 / 1 form, a twill 2 / 2 form, a twill 3 / 1 form, a satin 5S form or a satin 8S form; more preferably, the weaving form is a twill 2 / 2 form or a twill 3 / 1 form; Preferably, the total amount of the carbon fiber bundles in the functional fiber reinforcement is 3000 to 50000 strands; and / or the total amount of the linear phenolic fiber bundles is 1500 to 6000 strands.

4. A composite material, characterized in that: The raw materials for preparing the composite material include a flame retardant resin system for vacuum introduction and a functional fiber reinforcement according to any one of claims 1 to 3; Preferably, the mass ratio of the flame retardant resin system for vacuum introduction to the functional fiber reinforcement is 3.5:6.5 to 4.5:5.

5.

5. The composite material according to claim 4, characterized in that The flame retardant resin system for vacuum introduction comprises an epoxy resin component, a flame retardant resin component, a toughening resin component and a curing agent component; Preferably, the mass ratio of the epoxy resin component, the flame retardant resin component, the toughening resin component and the curing agent component is (49-51):(14-18):10:(23-25); Preferably, the flame retardant resin system for vacuum introduction has a viscosity of 400 cps to 1200 cps at 25°C.

6. The composite material according to claim 5, characterized in that The epoxy resin component includes epoxy resin; the epoxy resin includes at least one of bisphenol A epoxy resin and bisphenol F epoxy resin; Preferably, the epoxy resin component further comprises an epoxy reactive diluent; Preferably, the bisphenol A epoxy resin includes at least one of E-51 liquid resin, E-54 liquid resin, E-44 liquid resin and NPEL127 liquid resin; Preferably, the bisphenol F epoxy resin comprises NPEF-170 epoxy resin; Preferably, the epoxy reactive diluent includes at least one of XY622, XY699 and XY678.

7. The composite material according to claim 5, characterized in that The flame retardant resin component includes at least one of a second linear phenolic resin and a phosphorus-containing epoxy resin; Preferably, the melting point of the second linear phenolic resin is 60°C to 80°C; Preferably, the phosphorus-containing epoxy resin comprises at least one of a phosphorus-containing epoxy resin modified by phosphate ester and a phosphorus-containing epoxy resin modified by DOPO; Preferably, the phosphate-modified phosphorus-containing epoxy resin includes at least one of FR-633 and FR-7016; Preferably, the DOPO-modified phosphorus-containing epoxy resin includes at least one of D200, D201 and D202.

8. The composite material according to claim 5, characterized in that The toughening resin component includes at least one of polyurethane-modified epoxy resin, carboxyl-terminated nitrile rubber resin, dimer acid-modified epoxy resin and core-shell particle toughening resin containing nano rubber particles; Preferably, the polyurethane-modified epoxy resin comprises EPU133; Preferably, the carboxyl-terminated nitrile rubber resin includes at least one of CTBN1300X13, CTBN1300X8 and CTBN1300X31; Preferably, the dimer acid-modified epoxy resin comprises at least one of HyPox DA323 and YD-172; Preferably, the core-shell particle toughening resin containing nano rubber particles includes at least one of MX-962, MX-150 and MX-160.

9. The composite material according to claim 5, characterized in that The curing agent component includes at least one of a liquid acid anhydride curing agent and a modified liquid acid anhydride curing agent; Preferably, the curing agent component further comprises a liquid accelerator; Preferably, the modified liquid anhydride curing agent includes YEG-1070; Preferably, the liquid accelerator includes at least one of an imidazole-modified liquid accelerator and a complex-type liquid modifier.

10. A method for preparing a composite material according to any one of claims 4 to 9, characterized in that: The method comprises the following steps: vacuum-introducing a preform made of a functional fiber reinforcement and a flame-retardant resin system for vacuum induction, keeping the temperature at 95° C. to 120° C. for 1 h to 3 h, and then curing the preform at 130° C. to 150° C.; Preferably, the preparation of the preform comprises: laying the functional fiber reinforcement in a preset laying direction, and maintaining the preform under negative pressure at 90° C. to 100° C. for 20 min to 30 min.

Citation Information

Patent Citations

  • Continuous fiber reinforced thermosetting flame-retardant prepreg and preparation method thereof

    CN112625284A

  • Low-density ablation-resistant phenolic resin-based carbon fiber composite material and preparation method thereof

    CN116535811A

  • Carbon fiber reinforced composite material and production process thereof

    CN117445442A

  • Sizing agent, carbon fiber and carbon fiber-reinforced composite material

    JP2005320641A

  • Carbon riber and mesh structure tight processing carbon fiber prepreg and manufacturing method of the same

    KR1020180135203A