MOFs-copper-molybdenum bimetallic oxide / foamy copper array electrode material and preparation method and application thereof

By growing CuMoOx-HKUST-1 composite material on foamed copper substrate, using multi-interface and boundary effects, the problem of the activity changes of bimetallic oxide catalysts at high voltage is solved, and efficient electrocatalytic performance and stability are achieved. Electrocatalyzed in the oxygen evolution reaction.

CN119092307APending Publication Date: 2024-12-06ANHUI POLYTECHNIC UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411256894.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing bimetal oxide catalysts have problems with changes in the components and structure of active substances at high voltages, and the preparation of powdered electrocatalytic materials is complex and the electrocatalytic activity and stability are insufficient.

Method used

The CuMoOx precursor was grown on the foamed copper substrate by hydrothermal method, and CuMoOx-HKUST-1/CF composite was formed by high-temperature annealing and MOF modification, which improved catalytic activity and increased specific surface area and active sites by using multi-interface and boundary effects. Points.

Benefits of technology

It achieves stable electrocatalytic performance at high potential, improves electron conversion efficiency and stability, has better electrocatalytic activity and faster charge transfer rate, and is suitable for electrocatalysis of oxygen evolution reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092307A_ABST
    Figure CN119092307A_ABST
Patent Text Reader

Abstract

The invention provides an MOFs-copper molybdenum bimetallic oxide / foamy copper array electrode material and a preparation method and application thereof, and compared with the prior art, the MOFs-copper molybdenum bimetallic oxide / foamy copper array electrode material CuMoOx-HKUST-1 / CF is obtained by taking foamy copper (CF) as a carrier and adopting a hydrothermal method to prepare a CuMoOx precursor, then performing high-temperature annealing and finally performing modification by adopting porous MOF. The MOFs grown on the surface of the catalyst increase the contact area between the catalyst and an electrolyte, promote the diffusion of an electrolyte solution, provide more active sites, and have a faster charge transfer rate. The preparation method is simple, and the product and the performance are easy to repeat; the material has excellent electro-catalysis performance and has huge application potential in the field of electro-catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of new materials, and in particular relates to a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material and a preparation method and application thereof. Background Art

[0002] In recent years, a large number of studies have demonstrated that transition metal-based compounds have good electrocatalytic properties. In particular, transition metal oxides (TMOs) show particularly high catalytic activity and strong tolerance at high voltages. Bimetallic oxide catalysts can change the electronic structure of these catalysts by adjusting the metal composition and intrinsic activity. It is believed that bimetallic compounds provide abundant active sites, adsorb reaction intermediates, and improve the conductivity of the material.

[0003] At the same time, the porous structure of MOFs can make O 2 Rapid escape provides unique advantages for OER electrocatalytic reactions. Growing MOFs on the surface of metal oxides can form a large number of active sites and strong intermolecular forces, shortening the charge transfer path and increasing the utilization of active substances.

[0004] The patent with publication number CN 109205567 A published on January 15, 2019 discloses a method for preparing a multi-level structure of metal oxides using a MOF-derived bimetallic oxide template. 3 and 2-methylimidazole aqueous solution are dissolved in deionized water, a water-soluble salt solution of M is added, the mixture is heated to 80-180°C, stirred for reaction for more than 6 hours, cooled, washed and dried to obtain M / Mo-MOF material; the obtained M / Mo-MOF material is calcined at high temperature in an air atmosphere to obtain MMoO 4 -MOF-derived bimetallic oxides. However, no application of the products is disclosed. Summary of the invention

[0005] The object of the present invention is to provide a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material and a preparation method thereof, wherein a CuMoOx precursor is prepared by a hydrothermal method using foam copper (CF) as a carrier, and then high-temperature annealing is performed, and finally, a porous MOF is used for modification to obtain a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material CuMoOx-HKUST-1 / CF.

[0006] Another object of the present invention is to provide an application of a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material for electrocatalysis of oxygen evolution reaction. The electrode CuMoOx-HKUST-1 / CF composite material of the present invention grows MOFs on the surface of the metal oxide to form a large number of active sites and strong intermolecular forces, shortens the charge transfer path, increases the utilization of active substances, and as an electrocatalytic electrode for oxygen evolution reaction, improves the performance of electron conversion efficiency and stability, and has better electrocatalytic performance.

[0007] The specific technical solutions of the present invention are as follows:

[0008] A method for preparing a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material comprises the following steps:

[0009] 1) mixing phosphomolybdic acid hydrate, a copper source and urea in a solvent, adding copper foam, and performing a hydrothermal reaction to obtain a precursor;

[0010] 2) annealing the precursor obtained in step 1) at high temperature to obtain CuMoOx / CF;

[0011] 3) The organic ligand and the copper source are mixed in a solvent, and CuMoOx / CF is added to perform a solvothermal reaction to obtain CuMoOx-HKUST-1 / CF.

[0012] In step 1), the copper foam is pretreated before use; specifically, the copper foam is cut into 1 cm×2 cm pieces, the copper foam (CF) is ultrasonically cleaned with distilled water, ethanol and acetone respectively, and then dried in an oven at 60° C.;

[0013] In step 1), the atomic ratio of molybdenum in the phosphomolybdic acid hydrate to copper in the copper source is 2:1;

[0014] In step 1), the molar ratio of the phosphomolybdic acid hydrate to urea is 1:10;

[0015] In step 1), the amount ratio of the phosphomolybdic acid hydrate to the solvent is 0.01-0.015 mmol / L;

[0016] In step 1), the phosphomolybdic acid hydrate is H 3 Mo 12 O 40 P·xH 2 O, abbreviated as PMo 12 ;

[0017] In step 1), the copper source is selected from soluble copper salts, preferably copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O);

[0018] In step 1), the solvent is deionized water;

[0019] In step 1), the hydrothermal reaction refers to: 120° C., reaction time 15 h; through the hydrothermal method, the precursor forms a uniform array of microspheres on the surface of the copper foam, which has uniform size and regular morphology, and the diameter of the precursor microspheres is 9-10 μm.

[0020] In step 1), phosphomolybdic acid hydrate, copper source and urea are mixed in a solvent at room temperature;

[0021] In step 1), after the hydrothermal reaction is completed, the foam copper is washed with distilled water and ethanol to obtain an electrode precursor.

[0022] In step 2), the high temperature annealing is carried out in a nitrogen atmosphere at 300° C. for 2 h, and then naturally cooled to room temperature after the treatment.

[0023] In step 2), the high temperature annealing adopts a tubular furnace annealing reaction to achieve carbonization treatment.

[0024] In step 3), the molar ratio of the copper source to the organic ligand is 1:1;

[0025] In step 3), the amount ratio of the copper source to the solvent is 0.04-0.042 mmol / mL; during the solvent thermal synthesis, by controlling the Cu 2+ The concentration of CuMoOx / CF affects the specific morphology of the octahedral HKUST-1 grown on the surface of the CuMoOx / CF precursor.

[0026] In step 3), the organic ligand is 1,3,5-benzenetricarboxylic acid, C 9 H 6 O 6 , abbreviated as BTC;

[0027] In step 3), the copper source is selected from copper nitrate trihydrate;

[0028] Raw material copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O) provides a high-quality copper source for the synthesis of HKUST-1. 1,3,5-benzenetricarboxylic acid is used as a ligand to grow octahedral HKUST-1 on the surface of CuMoOx / CF precursor by hydrothermal method, which increases the specific surface area of ​​the catalyst.

[0029] In step 3), the solvent is an ethanol aqueous solution; in the ethanol aqueous solution, the volume ratio of ethanol to water is 1:1.

[0030] In step 3), the solvent thermal reaction refers to: 110° C., reaction time 24 h;

[0031] In step 3), the copper source and the organic ligand are mixed in a solvent at room temperature;

[0032] In step 3), after the solvothermal reaction is completed, the foam copper is washed with distilled water and ethanol to obtain the electrode CuMoOx-HKUST-1 / CF.

[0033] The present invention provides a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material, which is prepared by the above method. A micron sphere precursor is grown directly on a foam copper substrate by a hydrothermal method, and the diameter of the precursor micron sphere is 9-10 μm, and then 2 Three-dimensional football-shaped CuMoOx was obtained by annealing in an atmosphere. The pre-modified CuMoOx was used as the metal node and 1,3,5-benzenetricarboxylic acid was used as the organic ligand. Octahedral HKUST-1 with a size of 800±50nm was grown on its surface. The HKUST-1 prepared on the surface of copper foam had a uniform morphology and was not easy to fall off, thus constructing a MOFs-copper-molybdenum bimetallic oxide electrocatalyst.

[0034] The present invention uses copper foam as a base material to load copper-molybdenum bimetallic oxide as an active site. The bimetallic elements of multiple interfaces adjust the electronic structure under synergistic action, and the interface and boundary effects will greatly improve its catalytic activity, and the oxide can stably exist at a high potential to avoid changes in the active material components and structure. In addition, the copper foam substrate has good electrical conductivity, which is conducive to accelerating the transmission of electrons. In addition, the MOFs grown on the catalyst surface increase the contact area between the catalyst and the electrolyte, promote the diffusion of the electrolyte solution, provide more active sites, and have a faster charge transfer rate. Compared with the use of powdered electrocatalytic materials, the composite material grown in situ on the copper foam is directly used for the electrode, which not only avoids the use of a binder to facilitate the preparation of the electrode and is conducive to electron transmission, but also has more excellent electrocatalytic activity and stability than the powdered electrocatalytic material.

[0035] The present invention also provides an application of a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material for electrocatalysis of oxygen evolution reaction, and has excellent performance as an OER electrocatalytic material.

[0036] The inventors found that the multiple interfaces formed between active materials are beneficial to increase the number of active sites and enhance the adsorption of reaction intermediates due to their synergistic effects, boundary effects and interface interactions. Layered structures and electronic structure engineering are effective strategies to improve electrocatalytic performance. The layered structure has a higher specific surface area, increases the contact surface between the catalyst and the electrolyte, increases the number of exposed active sites, and is beneficial to electron conduction and proton transport. Therefore, the present invention designs a layered three-dimensional catalyst with multiple interfaces to improve electrocatalytic performance. Using the preparation method of the present invention, a multi-interface composite is obtained by modifying the surface of an array uniformly grown on copper foam by HKUST-1.

[0037] The present invention utilizes the characteristics of polyacid phosphomolybdic acid providing metal source and multi-interface porous structure of metal organic framework structure material, takes foam copper as substrate, and successfully prepares CuMoOx-HKUST-1 / CF array catalyst material through hydrothermal method, annealing and MOF modification method. In particular, MOFs grown on the surface of the catalyst increase the contact area between the catalyst and the electrolyte, promote the diffusion of the electrolyte solution, provide more active sites, and have a faster charge transfer rate. Moreover, the preparation method adopted by the present invention is simple, and the product and performance are easy to repeat; its excellent electrocatalytic performance has great application potential in the field of electrocatalysis.

[0038] Compared with the prior art, the present invention has the following beneficial effects: The present invention uses a hydrothermal method to prepare the precursor, which is simple, fast and easy to repeat. The preparation method of the present invention can obtain CuMoOx-HKUST-1 / CF, which is mainly characterized by HKUST-1 crystals with octahedral structure growing on the surface of the catalyst and evenly distributed on the foam copper skeleton. The CuMoOx-HKUST-1 / CF grown on the foam copper has better electrocatalytic performance. At a current density of 50 mA cm -2 When the overpotential is 290 mV, the current density is 100 mA cm -2 The overpotential is 368 mV. The sample also has excellent stability, and its LSV curve remains almost unchanged after 2000 cycles, making it an ideal catalyst for OER. The CuMoOx-HKUST-1 / CF composite material prepared by the present invention has great application potential in the field of electrocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a SEM image of the product of the present invention; wherein a is a SEM image of the CuMoOx precursor in Example 1; b is a SEM image of the CuMoOx precursor in Example 1 in N 2 a is the SEM image of CuMoOx / CF after annealing in atmosphere; c is the SEM image of the CuMoOx-HKUST-1 / CF-1 composite material in Example 1;

[0040] Figure 2 is the XRD diagram of the product of the present invention; wherein a is the XRD diagram of the CuMoOx precursor; b is the XRD diagram of N in Example 1 2 a is the XRD pattern of CuMoOx / CF after annealing in an atmosphere; c is the XRD pattern of the CuMoOx-HKUST-1 / CF-1 composite material in Example 1;

[0041] Figure 3 is the XPS photoelectron spectrum of the CuMoOx-HKUST-1 / CF-1 composite material in Example 1; wherein a is the full XPS spectrum of CuMoOx-HKUST-1 / CF-1; b is the XPS spectrum of C1s; c is the XPS spectrum of O1s; d is the spectrum of P 2p; e is the XPS spectrum of Mo 3d; f is the XPS spectrum of Cu 2p;

[0042] Figure 4 This is the EDS spectrum analysis diagram of the CuMoOx-HKUST-1 / CF-1 composite electrode material in Example 1;

[0043] Figure 5 is the SEM image of CuMoOx-HKUST-1 / CF-2 in Example 2;

[0044] Figure 6 is the SEM image of CuMoOx-HKUST-1 / CF-3 in Example 3;

[0045] Figure 7 is the SEM image of CuOx-HKUST-1 / CF in Example 4;

[0046] Figure 8 is the SEM image of MoOx-HKUST-1 / CF in Example 5;

[0047] Fig. 9 It is the OER curve of CuMoOx-HKUST-1 / CF-1, CuMoOx-HKUST-1 / CF-2, CuMoOx-HKUST-1 / CF-3, MoOx-HKUST-1 / CF, CuOx-HKUST-1 / CF and CuMoOx / CF;

[0048] Fig.10 It is the Tafel curve of CuMoOx-HKUST-1 / CF-1, CuMoOx-HKUST-1 / CF-2, CuMoOx-HKUST-1 / CF-3, MoOx-HKUST-1 / CF, CuOx-HKUST-1 / CF and CuMoOx / CF;

[0049] Fig.11are the cyclic voltammetry curves of CuMoOx-HKUST-1 / CF-1, CuMoOx-HKUST-1 / CF-2, CuMoOx-HKUST-1 / CF-3, MoOx-HKUST-1 / CF, CuOx-HKUST-1 / CF and CuMoOx / CF;

[0050] Fig.12 It is C of CuMoOx-HKUST-1 / CF-1, CuMoOx-HKUST-1 / CF-2, CuMoOx-HKUST-1 / CF-3, MoOx-HKUST-1 / CF, CuOx-HKUST-1 / CF and CuMoOx / CF dl Value graph;

[0051] Fig.13 This is the chronoamperometry diagram of CuMoOx-HKUST-1 / CF-1. DETAILED DESCRIPTION

[0052] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0053] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0054] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0055] The present invention provides a method for preparing a CuMoOx-HKUST-1 / CF-1 composite material, comprising the following steps:

[0056] 1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol, and acetone, respectively, and then dried in an oven at 60 °C. In a typical method, 0.1 mmol of phosphomolybdic acid hydrate (PMo) was added using continuous ultrasonication. 12 ), 0.6 mmol copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O) (Cu / Mo atomic ratio is 1:2) and 1mmol urea (Co(NH 2 ) 2) was dispersed in 10 mL of deionized water to obtain a uniform solution. The solution was transferred to a Teflonline stainless steel autoclave and immersed in the pretreated CF (1 cm × 2 cm), the autoclave was kept at 120 ° C for 15 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 ° C to obtain the CuMoOx precursor.

[0057] 2) Place the precursor from step 1) in a tube furnace at N 2 In the atmosphere, annealing was carried out at 300 °C for 2 h, and then naturally cooled to room temperature after carbonization treatment.

[0058] 3) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g (1 mmol) of 1,3,5-benzenetricarboxylic acid (BTC) was dissolved in a mixed solution of 12 mL of water and 12 mL of anhydrous ethanol, and ultrasonicated for 10 min. The solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene. The mixture prepared in step 2) was heated to 40 ℃ and then heated to 30 ℃. 2 The sample annealed in the atmosphere was immersed therein, and the autoclave was kept in an oven at 110°C for 24 h. The sample was taken out, washed with distilled water and anhydrous ethanol, and then dried in an oven at 60°C to prepare the CuMoOx-HKUST-1 / CF-1 sample.

[0059] The morphology of the CuMoOx-HKUST-1 / CF-1 composite material prepared by this method is mainly manifested in that the multi-interface MOFs material HKUST-1 increases the specific surface area and the number of active sites of CuMoOx-HKUST-1 / CF-1, and the octahedral structure of HKUST-1 grows uniformly on the surface of the CuMoOx-HKUST-1 / CF-1 catalyst.

[0060] The following is a detailed description through several specific embodiments:

[0061] Example 1

[0062] A method for preparing a CuMoOx-HKUST-1 / CF-1 composite material comprises the following steps:

[0063] 1) Preparation of precursor composite materials:

[0064] 1-1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol and acetone, and then dried in an oven at 60°C;

[0065] 1-2) Copper-molybdenum atomic ratio Cu / Mo=1:2, 0.1mmol phosphomolybdic acid hydrate (PMo12), 0.6mmol copper nitrate trihydrate (Cu(NO 3 )2 ·3H 2 O) and 1 mmol urea (Co(NH 2 ) 2 ) were dispersed in 10 mL of deionized water solution and continuous ultrasound was used to obtain a homogeneous solution;

[0066] 1-3) keeping the autoclave at 120°C for 15h, then cooling naturally to room temperature, washing with distilled water and ethanol and drying in an oven at 60°C;

[0067] 1-4) Place it in a tube furnace at N 2 The CuMoOx / CF was obtained by annealing at 300 °C for 2 h in a carbonized atmosphere and naturally cooling to room temperature.

[0068] 2) Preparation of CuMoOx-HKUST-1 / CF-1 composite materials:

[0069] 2-1) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g (1 mmol) of 1,3,5-benzenetricarboxylic acid (BTC) was dissolved in a mixed solution of 12 mL of water and 12 mL of anhydrous ethanol, and ultrasonicated for 10 min;

[0070] 2-2) will be in N 2 The sample annealed in atmosphere was immersed in an autoclave and kept at 110 °C for 24 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 °C to prepare the CuMoOx-HKUST-1 / CF-1 sample.

[0071] Scanning electron microscopy (SEM), X-ray diffraction (XRD), X-ray photoelectron diffraction (XPS) and energy dispersive spectroscopy (EDS) were used to characterize the CuMoOx precursor, 2 The morphology and structure of CuMoOx / CF, CuMoOx-HKUST-1 / CF-1 and related samples after annealing in atmosphere were characterized, and the electrochemical performance of related electrode oxygen evolution reaction (OER) was tested and analyzed.

[0072] The results are as follows Figure 1 As shown, Figure 1 Figure a is a SEM image of the CuMoOx precursor in Example 1. From the image, it can be seen that the foamed copper is covered with spherical precursors with smooth surfaces. Figure 1 b is the value of N in Example 1 2 The locally enlarged SEM image of CuMoOx / CF after annealing in atmosphere shows that it becomes a football-shaped morphology after annealing and shows a regular plane. Figure 1Figure c is a SEM image of CuMoOx-HKUST-1 / CF-1 in Example 1. It can be seen from the figure that octahedral HKUST-1 crystals grow on the surface of the catalyst.

[0073] Figure 2 The XRD spectrum of CuMoOx precursor is shown in a, showing Cu at 36.3°, 42.5°, 61.2° and 73.3°. 2 O (JCPDS 05-0667) characteristic peaks and foam copper Cu (JCPDS 04-0836) characteristic peaks at 43.5°, 50.7°, and 74.4°. Figure 2 b is N 2 The XRD pattern of CuMoOx / CF after annealing in atmosphere shows that the diffraction peaks at 21.8°, 24.3°, 25.8°, 32.2°, 47.7°, 53.6°, 61.3°, and 77.1° correspond to MoO 3 The characteristic peaks of (JCPDS 01-0706), and the other characteristic peaks correspond to Cu 2 O and copper foam. The XRD spectrum of CuMoOx-HKUST-1 / CF-1 is shown in Figure 2 As shown in c, MoO 3 , Cu 2 O, Cu and HKUST-1 characteristic peaks (6.7, 10.4, 11.6, 13.4 and 18.9°), which further proves that Cu 2 O、MoO 3 The successful preparation of HKUST-1 on copper foam and the successful composite of CuMoOx / CF and HKUST-1. In addition, in order to further characterize the composition and properties of CuMoOx-HKUST-1 / CF-1, the following tests were carried out.

[0074] By using XPS characterization, we further understood the chemical composition and element valence state of the CuMoOx-HKUST-1 / CF-1 catalyst surface. Figure 3 As shown in Figure a, the XPS spectrum of CuMoOx-HKUST-1 / CF-1 shows that it mainly contains C, O, P, Mo and Cu elements. Figure 3 Figure b shows the XPS spectrum of C1s, where three different C1s signals are observed. The CC bond of the benzene ring in the BTC ligand is responsible for the peak observed at 284.9 eV, the presence of CO / C-OH species can explain the peak observed at 286 eV, and the peak at 288.5 eV can be attributed to the formation of C=O. Figure 3 The signals of the XPS spectrum of O1s in c at 531.6 and 532.5 eV are Mo-O and HOH bonds, respectively; Figure 3 The spectrum of P 2p in d contains peaks at 133 and 134.2 eV, which correspond to the PO bonds in phosphate. Figure 3 Figure e shows the Mo 3d XPS spectrum of CuMoOx-HKUST-1 / CF-1. The peaks at 232.3 eV and 235.4 eV correspond to the Mo 3d 5 / 2 and Mo 3d 3 / 2 , which shows that Mo 6+ Figure f shows the XPS spectrum of Cu 2p, from which it can be seen that the binding energies of CuMoOx-HKUST-1 / CF-1 at 934.4 eV and 954.7 eV correspond to Cu 2+ Cu 2p 3 / 2 and Cu 2p 1 / 2 The peaks at 932.4eV and 952.5eV correspond to Cu + Cu 2p 3 / 2 and Cu 2p 1 / 2 In addition, the three satellite peaks at 941.2eV, 943.3eV and 962.5eV are Cu 2+ and Cu + obvious characteristics. Figure 4 It is the energy dispersion spectrum of CuMoOx-HKUST-1 / CF-1, which further verifies the existence of C, O, P, Cu, and Mo elements in CuMoOx-HKUST-1 / CF-1.

[0075] Example 2 (for comparison)

[0076] A method for preparing a CuMoOx-HKUST-1 / CF-2 composite material comprises the following steps:

[0077] 1) Preparation of Precursor-2 Composite Material:

[0078] 1-1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol and acetone, and then dried in an oven at 60°C;

[0079] 1-2) Copper-molybdenum atomic ratio Cu / Mo=1:1, 0.1mmol phosphomolybdic acid hydrate (PMo 12 ), 1.2mmol copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O) and 1 mmol urea (Co(NH 2 ) 2 ) were dispersed in 10 mL of deionized water solution and continuous ultrasound was used to obtain a homogeneous solution;

[0080] 1-3) keeping the autoclave at 120°C for 15h, then cooling naturally to room temperature, washing with distilled water and ethanol and drying in an oven at 60°C;

[0081] 1-4) Place it in a tube furnace at N 2 In the atmosphere, annealing was carried out at 300 °C for 2 h, and then naturally cooled to room temperature after carbonization treatment.

[0082] 2) Preparation of CuMoOx-HKUST-1 / CF-2 composite materials:

[0083] 2-1) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g (1 mmol) of 1,3,5-benzenetricarboxylic acid (BTC) was dissolved in a mixed solution of 12 mL of water and 12 mL of anhydrous ethanol, and ultrasonicated for 10 min;

[0084] 2-2) will be in N 2 The sample annealed in atmosphere was immersed in an autoclave and kept at 110 °C for 24 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 °C to prepare the CuMoOx-HKUST-1 / CF-2 sample.

[0085] CuMoOx-HKUST-1 / CF-2 was analyzed by scanning electron microscopy (SEM).

[0086] like Figure 5 As shown, Figure 5 This is the SEM image of CuMoOx-HKUST-1 / CF-2 in Example 2. It can be seen from the figure that the HKUST-1 grown on the foam copper has an irregular morphology and a large number of aggregates appear in some areas. This is due to the Cu 2+ Too high a concentration will result in excessive accumulation of crystals.

[0087] Example 3 (for comparison)

[0088] A method for preparing a CuMoOx-HKUST-1 / CF-3 composite material comprises the following steps:

[0089] 1) Preparation of Precursor-3 Composite Material:

[0090] 1-1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol and acetone, and then dried in an oven at 60°C;

[0091] 1-2) Copper-molybdenum atomic ratio Cu / Mo=1:3, 0.1mmol phosphomolybdic acid hydrate (PMo 12), 0.4mmol copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O) and 1 mmol urea (Co(NH 2 ) 2 ) were dispersed in 10 mL of deionized water solution and continuous ultrasound was used to obtain a homogeneous solution;

[0092] 1-3) keeping the autoclave at 120°C for 15h, then cooling naturally to room temperature, washing with distilled water and ethanol and drying in an oven at 60°C;

[0093] 1-4) Place it in a tube furnace at N 2 In the atmosphere, annealing was carried out at 300 °C for 2 h, and then naturally cooled to room temperature after carbonization treatment.

[0094] 2) Preparation of CuMoOx-HKUST-1 / CF-3 composite materials:

[0095] 2-1) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g (1 mmol) of 1,3,5-benzenetricarboxylic acid (BTC) was dissolved in a mixed solution of 12 mL of water and 12 mL of anhydrous ethanol, and ultrasonicated for 10 min;

[0096] 2-2) will be in N 2 The sample calcined under atmosphere was immersed in an autoclave and kept at 110 °C for 24 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 °C to prepare the CuMoOx-HKUST-1 / CF-3 sample.

[0097] CuMoOx-HKUST-1 / CF-3 was analyzed by scanning electron microscopy (SEM).

[0098] like Figure 6 As shown, Figure 6 This is the SEM image of CuMoOx-HKUST-1 / CF-3 in Example 3. It can be seen from the figure that when the content of metal source Cu is low, the HKUST-1 grown on the foam copper is disordered and irregular. This is because Cu 2+ Too low a concentration results in very uneven crystal formation.

[0099] Example 4 (for comparison)

[0100] A method for preparing a CuOx-HKUST-1 / CF composite material comprises the following steps:

[0101] 1) Preparation of Precursor-4 Composite Material:

[0102] 1-1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol and acetone, and then dried in an oven at 60°C;

[0103] 1-2) 0.6 mmol of copper nitrate trihydrate (Cu(NO 3 ) 2 ·3H 2 O) and 1 mmol urea (Co(NH 2 ) 2 ) were dispersed in 10 mL of deionized water solution and continuous ultrasound was used to obtain a homogeneous solution;

[0104] 1-3) keeping the autoclave at 120°C for 15h, then cooling naturally to room temperature, washing with distilled water and ethanol and drying in an oven at 60°C;

[0105] 1-4) Place it in a tube furnace at N 2 In the atmosphere, annealing was carried out at 300 °C for 2 h, and then naturally cooled to room temperature after carbonization treatment.

[0106] 2) Preparation of CuOx-HKUST-1 / CF composite materials:

[0107] 2-1) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g BTC was dissolved in a mixed solution of 12 mL water and 12 mL anhydrous ethanol, and ultrasonicated for 10 min;

[0108] 2-2) will be in N 2 The sample calcined under atmosphere was immersed in an autoclave and kept at 110 °C for 24 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 °C to prepare the CuOx-HKUST-1 / CF sample.

[0109] CuOx-HKUST-1 / CF was analyzed by scanning electron microscopy (SEM).

[0110] like Figure 7 As shown, Figure 7 This is the SEM image of CuOx-HKUST-1 / CF in Example 4. It can be seen from the figure that when the metal source is only Cu, the HKUST-1 grown on the foam copper is unevenly distributed, and a small amount of aggregation appears in some areas. This is because Cu 2+ Too high a concentration results in dense crystal formation.

[0111] Example 5 (for comparison)

[0112] A method for preparing a MoOx-HKUST-1 / CF composite electrode material comprises the following steps:

[0113] 1) Preparation of Precursor-5 Composite Electrode:

[0114] 1-1) The copper foam was cut into 1 cm × 2 cm pieces, and the copper foam (CF) was ultrasonically cleaned with distilled water, ethanol and acetone, and then dried in an oven at 60°C;

[0115] 1-2) 0.1 mmol of phosphomolybdic acid hydrate (PMo 12 ) and 1mmol urea (Co(NH 2 ) 2 ) were dispersed in 10 mL of deionized water solution and continuous ultrasound was used to obtain a homogeneous solution;

[0116] 1-3) keeping the autoclave at 120°C for 15h, then cooling naturally to room temperature, washing with distilled water and ethanol and drying in an oven at 60°C;

[0117] 1-4) Place it in a tube furnace at N 2 In the atmosphere, annealing was carried out at 300 °C for 2 h, and then naturally cooled to room temperature after carbonization treatment.

[0118] 2) Preparation of MoOx-HKUST-1 / CF composite materials:

[0119] 2-1) 1mmol Cu(NO 3 ) 2 ·3H 2 O, 0.21 g BTC was dissolved in a mixed solution of 12 mL water and 12 mL anhydrous ethanol, and ultrasonicated for 10 min;

[0120] 2-2) will be in N 2 The sample calcined under atmosphere was immersed in an autoclave and kept at 110 °C for 24 h, then naturally cooled to room temperature, washed with distilled water and ethanol and dried in an oven at 60 °C to prepare the CuOx-HKUST-1 / CF sample.

[0121] Scanning electron microscopy (SEM) was used to analyze MoOx-HKUST-1 / CF.

[0122] like Figure 8 As shown, Figure 8 This is the SEM image of MoOx-HKUST-1 / CF in Example 5. It can be seen from the figure that the MoOx-HKUST-1 / CF synthesized without adding additional copper source has too low copper content and no regular HKUST-1 octahedral morphology can be seen on its surface.

[0123] Example 6

[0124] The three-electrode system was used to test the electrochemical performance of CuMoOx-HKUST-1 / CF-1 prepared in Example 1, the precursor CuMoOx / CF prepared in Example 1, the CuMoOx-HKUST-1 / CF-2 prepared in Example 2, the CuMoOx-HKUST-1 / CF-3 prepared in Example 3, the CuOx-HKUST-1 / CF prepared in Example 4, and the MoOx-HKUST-1 / CF prepared in Example 5 as working electrodes. The specific operation is as follows: the copper foam, graphite rod and saturated Ag / AgCl electrode loaded with samples prepared in each example were used as the working electrode, counter electrode and reference electrode, respectively, and the electrolyte was 1 mol·L -1 The electrochemical performance was tested and analyzed using an electrochemical workstation (CHI660E).

[0125] First, the samples were tested by linear sweep voltammetry (LSV) at a scan rate of 5 mV·s -1 The polarization curve of the sample is obtained. The Tafel slope of the sample is fitted and calculated based on the polarization curve data. In the voltage range of 0.2 to 0.3 V, different scan rates such as 20 mV·s -1 , 40mV·s -1 、60mV·s -1 、80mV·s -1 , 100mV·s -1 , 120mV·s -1 , 140mV·s -1 The cyclic voltammetry curve of the sample under the condition of 1.52V was fitted to obtain the electrochemical specific surface area data. The current density stability curve of the electrode was obtained by using the chronoamperometry method with the voltage kept at 1.52V.

[0126] like Fig. 9 The polarization curves show that the CuMoOx-HKUST-1 / CF-1 composite material has better electrocatalytic activity. -2 When the potential of CuMoOx-HKUST-1 / CF-1 is 1.52V, the formula η=E RHE-1.23 calculation shows that at this current density, the overpotential of CuMoOx-HKUST-1 / CF-1 is 290mV, which is significantly lower than 345mV of CuMoOx / CF precursor, 438mV of CuMoOx-HKUST-1 / CF-2, 377mV of CuMoOx-HKUST-1 / CF-3, 538mV of CuOx-HKUST-1 / CF and 427mV of MoOx-HKUST-1 / CF. The bimetallic oxides have excellent synergistic effects and strong adsorption of active intermediates and easy desorption of oxygen. The unique three-dimensional structure and high conductivity of the copper foam substrate and the porous structure of MOFs can make O 2 Rapid escape provides unique advantages for OER electrocatalytic reactions. The above factors work together to improve the electrocatalytic activity of the material.

[0127] Tafel slope is an important method for studying the kinetics of catalytic reactions of electrocatalytic materials. Its value can be obtained by simulating and calculating the LSV curve using the Tafel equation. Specifically, log(j) in the catalyst LSV curve is used as the horizontal coordinate and its overpotential is used as the vertical coordinate. Based on the LSV test data of CuMoOx-HKUST-1 / CF-1, CuMoOx-HKUST-1 / CF-2, CuMoOx-HKUST-1 / CF-3, CuMoOx / CF precursor, CuOx-HKUST-1 / CF and MoOx-HKUST-1 / CF, their Tafel slopes are calculated respectively. The results are as follows: Fig.10 It can be seen that the Tafel slope of CuMoOx-HKUST-1 / CF-1 is the lowest, which is 109.05mV dec. -1 , which is lower than CuMoOx-HKUST-1 / CF-2 (373.25mV dec -1 ), CuMoOx-HKUST-1 / CF-3(218.78mV dec -1 ), CuOx-HKUST-1 / CF(539.35mV dec -1 ), MoOx-HKUST-1 / CF(349.65mV dec -1 ) and CuMoOx / CF (171.36mV dec -1 ). The results show that CuMoOx-HKUST-1 / CF-1 has high catalytic kinetic activity, which may be due to the relatively uniform growth of MOFs on the surface of copper foam, which increases the specific surface area of ​​the catalyst, increases the number of active sites, promotes the rapid transfer of charges, and has excellent kinetic activity.

[0128] An important indicator of the catalytic activity of electrocatalysts is the electrochemically active surface area, which was investigated by combining cyclic voltammetry and electrochemical double layer capacitance. -1 -140mV s -1 ) and the cyclic voltammetry curves of each catalyst were measured in the non-Faraday region of 0.2-0.3 V. Fig.11 ). Fig.12 The horizontal axis represents different scan rates, and the vertical axis represents the current density difference of the CV data at different scan rates. The data is fitted according to the relationship between the horizontal and vertical axes, and the slope of the two straight lines is the double-layer capacitance value (C dl ). It can be seen from the fitting that the C of CuMoOx-HKUST-1 / CF-1 dl The value is 15.3mF cm -2 , greater than CuMoOx / CF (4.2mF cm -2 ), CuMoOx-HKUST-1 / CF-3(2.1mF cm -2 ), CuMoOx-HKUST-1 / CF-2(1.3mF cm -2 )、MoOx-HKUST-1 / CF(1.4mF cm -2 ) and CuOx-HKUST-1 / CF(0.35mFcm -2 ), which shows that the CuMoOx-HKUST-1 / CF-1 sample has the largest ECSA and the best OER activity, which is consistent with the SEM image and LSV test. The results prove that CuMoOx-HKUST-1 / CF-1 has a larger catalytic active specific surface area, which can expose more active sites, so its OER performance is also significantly improved.

[0129] The stability of the electrode material of Example 1 was determined by chronoamperometry with a voltage of 1.52 V. After 12 h of continuous testing, Fig.13 It can be seen that the LSV polarization curve after 2000 CV cycles is only slightly offset compared with the curve before the cycle, indicating that CuMoOx-HKUST-1 / CF-1 stably maintains the catalytic activity of the electrode material after the OER reaction. First, the bimetallic oxide has good stability at high potentials and the structure of the active site does not change; secondly, the synergistic effect of CuMoOx and HKUST-1 can accelerate the charge transfer rate. The electron transfer in this structure promotes the adsorption and activation of water molecules, which is conducive to the dissociation and generation of O 2 , thereby improving the intrinsic kinetics of the OER process.

[0130] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material, characterized in that: The preparation method comprises the following steps: 1) mixing phosphomolybdic acid hydrate, a copper source and urea in a solvent, adding copper foam, and performing a hydrothermal reaction to obtain a precursor; 2) annealing the precursor obtained in step 1) at high temperature to obtain CuMoOx / CF; 3) The organic ligand and the copper source are mixed in a solvent, and CuMoOx / CF is added to perform a solvothermal reaction to obtain CuMoOx-HKUST-1 / CF.

2. The preparation method according to claim 1, characterized in that: In step 1), the atomic ratio of molybdenum in the phosphomolybdic acid hydrate to copper in the copper source is 2:

1.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1), the molar ratio of the phosphomolybdic acid hydrate to urea is 1:

10.

4. The preparation method according to claim 1 or 2, characterized in that: In step 1), the solvent is deionized water; the hydrothermal reaction is carried out at 120° C. for 15 hours.

5. The preparation method according to claim 1, characterized in that: In step 2), the high temperature annealing is carried out in a nitrogen atmosphere at 300° C. for 2 h.

6. The preparation method according to claim 1, characterized in that: In step 3), the molar ratio of the copper source to the organic ligand is 1:

1.

7. The preparation method according to claim 1 or 6, characterized in that: In step 3), the solvent is an ethanol aqueous solution; in the ethanol aqueous solution, the volume ratio of ethanol to water is 1:

1.

8. The preparation method according to claim 1 or 6, characterized in that: In step 3), the solvent thermal reaction refers to: 110° C., reaction time 24 h.

9. A MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the MOFs-copper-molybdenum bimetallic oxide / foam copper array electrode material according to claim 9, characterized in that: Used for electrocatalysis of oxygen evolution reaction.

Citation Information

Patent Citations

  • Method for preparing metal oxide multistage structure by MOF-derived bimetallic oxide template

    CN109205567A