Novel zinc ion conductive additive modified capacitive electrode and preparation method thereof
By adding zinc trifluoromethanesulfonate and acrylamide to the activated carbon electrode to form a floc complex, and combining conductive additives, the problems of low energy density and conductivity of activated carbon capacitors are solved, and high capacity and high energy density are achieved The preparation of zinc ion hybrid capacitor electrode materials simplifies the process and improves performance.
Patent Information
- Application Number
- CN202411481470.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-12-06
AI Technical Summary
The low energy density and low conductivity of existing activated carbon capacitors limit the charge transport performance of zinc ion hybrid capacitors.
By mixing zinc trifluoromethanesulfonate and acrylamide with activated carbon, a floc complex is formed, and the conductive carbon black and polyvinylidene fluoride is combined with the solution casting method to prepare electrode materials to increase the adsorption capacity of zinc ions and electrodes ion conductivity.
It significantly improves the capacity, rate performance and energy density of the electrode, simplifies the preparation process, and realizes the preparation of electrode materials for high-performance zinc ion hybrid capacitors, and the process is simple and environmentally friendly.
Smart Images

Figure CN119092310A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a novel capacitor electrode modified by a zinc ion conductive auxiliary agent and a preparation method thereof, belonging to the technical field of capacitor materials. Background Art
[0002] Zinc ion hybrid capacitors (ZIHCs) are a new type of energy storage device, which usually consists of a zinc anode, a porous carbon cathode and a Zn 2+ The hybrid capacitor was developed to make up for the lack of performance of individual batteries or supercapacitors. It combines the advantages of zinc-ion batteries and supercapacitors, with high energy density and high power density, while maintaining long cycle life and excellent safety performance.
[0003] The electrode materials of ZIHCs can be classified into two categories: capacitive materials and battery materials. Capacitive electrode materials provide better rate performance and cycle stability for the adsorption / desorption of zinc ions, but capacitive electrode materials play a vital role in ZIHCs. They are usually porous carbon materials with high specific area and optimized pore structure to increase the contact area with the electrolyte and provide a fast ion transport path. These materials include but are not limited to commercial activated carbon (AC), carbon nanotubes, graphene, and porous carbon.
[0004] Generally, activated carbon as capacitor electrode has the characteristics of good electrochemical stability and environmental friendliness, but its disadvantages are also very obvious. The low energy density of activated carbon positive electrode and the low conductivity of activated carbon itself have certain limitations on charge transfer. Therefore, it is very necessary to provide a capacitive electrode for zinc ion hybrid capacitor with simple preparation method and excellent electrochemical performance. Summary of the invention
[0005] In view of the current status of low energy density of existing activated carbon capacitors and low conductivity of activated carbon itself, the present invention provides a novel capacitor electrode modified with a zinc ion conductive additive and a preparation method thereof.
[0006] The technical solution of the present invention:
[0007] The preparation method of the novel high-capacity and high-energy-density zinc ion hybrid capacitor electrode is as follows:
[0008] Step 1, adding activated carbon of different weights, zinc trifluoromethanesulfonate, and acrylamide to N-methylpyrrolidone, adding an appropriate amount of conductive carbon black and 7wt% polyvinylidene fluoride, and stirring on a magnetic stirrer for 5 hours until the activated carbon is evenly dispersed and the additives are fully dissolved to obtain an electrode precursor solution;
[0009] Step 2, coating the electrode precursor solution treated in step 1 onto the current collector using a coating machine and a scraper to obtain an electrode precursor;
[0010] Step 3, drying the electrode precursor obtained after the treatment in step 2 in a vacuum oven for a period of time until the solution is completely volatilized to obtain an electrode sheet;
[0011] Step 4, cutting, weighing and labeling the electrode obtained in step 3 on a cutting machine to obtain electrode discs;
[0012] Step 5, placing the electrode sheet obtained in step 4 into a vacuum oven for drying for a period of time to obtain a zinc ion hybrid capacitor electrode.
[0013] Furthermore, in step 1, the main body of the mixture is activated carbon, wherein the mass ratio of activated carbon, zinc trifluoromethanesulfonate and acrylamide is 150:(3-7):(3-7).
[0014] Furthermore, in step 1, the rotation speed and temperature of the magnetic stirrer are 600 r / min and 25° C. respectively.
[0015] Furthermore, in step 2, the current collector coated with the electrode precursor solution is one of carbon paper, carbon cloth, graphite paper, stainless steel foil, stainless steel mesh, and titanium foil.
[0016] Furthermore, in step 2, the thickness of the electrode precursor coated is 180 μm-190 μm.
[0017] Furthermore, in step three, the vacuum oven drying conditions are: oven temperature 80° C., and drying time 12 h.
[0018] Furthermore, the size of the cut pieces in step 4 is a disc with a diameter of 12 mm, and the mass of active material in the electrode calculated after weighing is 0.6 mg-2.5 mg.
[0019] Furthermore, in step 5, the vacuum oven drying conditions are: oven temperature 80° C., and drying time 2 h.
[0020] Furthermore, the preparation method of this patent is only a solution casting method, and does not use complex methods such as ball milling.
[0021] The present invention has the following beneficial effects: The present invention uses a solution casting method to prepare an electrode material that achieves the purpose by adjusting variables such as the content of additives, the type of current collector, and the thickness of the coating film. It has the following advantages:
[0022] (1) Through the interaction between zinc trifluoromethanesulfonate and acrylamide, acrylamide and zinc ions form flocculent complexes in activated carbon, which increases the adsorption capacity of the electrode material for zinc ions, increases the electrode wettability, and helps the penetration of the electrolyte and ion transport. Compared with the original activated carbon electrode, the capacity is significantly improved. By adjusting the content of additives, the reversible capacity, rate performance and energy density are further improved.
[0023] (2) The introduced mixture of zinc trifluoromethanesulfonate and acrylamide serves as a new conductive additive to improve the ion conductivity of the electrode itself and provide a feasible solution for high-performance zinc ion hybrid capacitors.
[0024] (3) Through the selection of current collectors and the regulation of coating thickness, the compatibility between current collectors and electrode materials, as well as the most suitable surface density of active materials, is explored, and the optimal solution is selected through experiments.
[0025] (4) Only by solution casting, our electrode preparation process is simple, the preparation cycle is short, and the repeatability is high. At the same time, the preparation process is simple, the flow is clear, and it is green and pollution-free, which is more suitable for the practical application of this zinc ion hybrid capacitor electrode and provides an idea for the pollution-free preparation of high energy density electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The EIS graph of the zinc ion hybrid capacitor using YP-50F activated carbon and YP-50F activated carbon modified with a conductive additive as electrodes prepared in the example;
[0027] Figure 2 The charge and discharge curves of the zinc ion hybrid capacitor assembled with the electrodes prepared in the example at different current densities, wherein (a) is a YP-50F activated carbon electrode, and (b) is a YP-50F activated carbon electrode modified with a conductive additive;
[0028] Figure 3 The multiplier test curve of the zinc ion hybrid capacitor using YP-50F activated carbon and YP-50F activated carbon modified with a conductive additive as electrodes prepared in the example;
[0029] Figure 4 The long cycle performance curve of the zinc ion hybrid capacitor using YP-50F activated carbon and YP-50F activated carbon modified with a conductive additive as electrodes prepared in the example. DETAILED DESCRIPTION
[0030] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0031] Embodiment 1:
[0032] Preparation process of activated carbon YP-50F electrode material:
[0033] (1) 0.15 g of YP-50F activated carbon and 0.02 g of conductive carbon black were put into a mortar and ground for 30 min, 0.26 g of 7 wt% polyvinylidene fluoride was added, and an appropriate amount of N-methylpyrrolidone was added dropwise. The mixture was stirred at 600 r / min and 25 °C for 5 h using a magnetic stirrer until the activated carbon was evenly dispersed and the additives were fully dissolved.
[0034] (2) The precursor solution in (1) is coated onto carbon paper using a coating machine and a doctor blade, and the obtained electrode precursor has a thickness of about 187 μm.
[0035] (3) The electrode precursor coated in (2) is placed in a vacuum oven, heated to 80° C., and allowed to stand for 12 h.
[0036] (4) Cut the electrode sheet treated in (3) into 12 mm round pieces and weigh them separately.
[0037] (5) Heat the disc in (4) in a vacuum oven to 80°C, let it stand for 2 h, and put it into a sealed bag for later use.
[0038] Preparation process of modified YP-50F electrode material: The difference from the preparation process of activated carbon YP-50F electrode material is that 5 mg of zinc trifluoromethanesulfonate and 5 mg of acrylamide are additionally added. The rest of the steps are the same, and finally the modified YP-50F electrode material is obtained.
[0039] The performance of the capacitive electrode of the high-performance zinc ion hybrid capacitor modified with the conductive additive prepared in Example 1 was characterized, and the results are as follows:
[0040] Figure 1 This is the EIS graph of the zinc ion hybrid capacitor with YP-50F activated carbon and YP-50F activated carbon modified with conductive additive as electrodes. It can be seen from the figure that the modified battery shows lower impedance than before modification.
[0041] Figure 2 The charge and discharge curves of zinc ion hybrid capacitors assembled with YP-50F activated carbon and YP-50F activated carbon modified with conductive additive as electrodes at different current densities. It can be seen from the figure that at the same current density, the zinc ion hybrid capacitor assembled with the electrode modified with conductive additive has a higher capacity.
[0042] Figure 3This is the rate test curve of zinc ion hybrid capacitor with YP-50F activated carbon and YP-50F activated carbon modified with conductive additive as electrodes. However, after high current charging, the capacity of the zinc ion hybrid capacitor made of the modified electrode has a certain degree of decrease compared with the capacity before experiencing high current. The high current tolerance of the modified electrode is slightly lower than that of the electrode before modification. Both electrodes have good rate performance.
[0043] Figure 4 The long cycle performance curves of zinc ion hybrid capacitors with YP-50F activated carbon and YP-50F activated carbon modified with conductive additive as electrodes. Both electrodes remain stable within 200 cycles, and the cycle efficiency is close to 100%, but the capacity of the zinc ion hybrid capacitor with YP-50F activated carbon modified with conductive additive as electrode reaches 138F g -1 The capacity of zinc ion hybrid capacitor with YP-50F activated carbon as electrode is only 80F g -1 , the capacity retention rates of both are close to 100%.
Claims
1. A novel capacitive electrode modified with a zinc ion conductive additive, characterized in that: The electrode is a zinc ion hybrid capacitor cathode composed of activated carbon as the main body and zinc trifluoromethanesulfonate and acrylamide as additives. The effect of additives of different qualities on the performance of the activated carbon electrode is explored. The electrode invented and verified the optimization mechanism of zinc trifluoromethanesulfonate and acrylamide on the capacity and energy density of the zinc ion hybrid capacitor.
2. The method for preparing a novel zinc ion conductive additive modified capacitive electrode according to claim 1, characterized in that: The method steps are as follows: Step 1, adding activated carbon of different weights, zinc trifluoromethanesulfonate, and acrylamide to N-methylpyrrolidone, adding an appropriate amount of conductive carbon black and 7wt% polyvinylidene fluoride, and stirring on a magnetic stirrer for 5 hours until the activated carbon is evenly dispersed and the additives are fully dissolved to obtain an electrode precursor solution; Step 2, coating the electrode precursor solution treated in step 1 onto the current collector using a coating machine and a scraper to obtain an electrode precursor; Step 3, drying the electrode precursor obtained after the treatment in step 2 in a vacuum oven for a period of time until the solution is completely volatilized to obtain an electrode sheet; Step 4, cutting, weighing and labeling the electrode sheet obtained in step 3 on a cutting machine to obtain electrode discs; Step 5, placing the electrode disc obtained in step 4 into a vacuum oven for drying for a period of time to obtain a zinc ion hybrid capacitor electrode.
3. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: In the step 1, the active substance is activated carbon, and the additives are zinc trifluoromethanesulfonate and acrylamide, wherein the mass ratio of activated carbon, zinc trifluoromethanesulfonate and acrylamide is 150:(3-7):(3-7).
4. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: The current collector for coating the precursor in step 2 is one of carbon paper, carbon cloth, graphite paper, stainless steel foil, stainless steel mesh, and titanium foil.
5. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: The thickness of the coating precursor in the step 2 is 180 μm-190 μm.
6. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: After weighing in step 4, the mass of active material in the electrode is calculated to be 0.6 mg-2.5 mg.
7. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: The purpose of step five is to dry the moisture in the air adsorbed during the weighing process of the cut pieces.
8. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: Acrylamide and zinc trifluoromethanesulfonate are added as conductive additives and introduced into activated carbon. Flocculent complexes are formed in the activated carbon, which enhances its adsorption capacity for ions in the electrolyte, improves the conductivity of the electrode, and improves the charge transfer characteristics.
9. The method for preparing a novel zinc ion conductive additive-modified capacitive electrode according to claim 2, characterized in that: Different from other invention patents, this patent develops the application of acrylamide and zinc trifluoromethanesulfonate as conductive additives to increase the ionic conductivity of zinc ion hybrid capacitors.
10. The method for preparing a novel capacitive electrode modified with a zinc ion conductive additive according to claim 2, characterized in that: This patent studies the interaction mechanism between activated carbon, acrylamide and zinc trifluoromethanesulfonate, and invents and verifies the optimization mechanism of zinc trifluoromethanesulfonate and acrylamide on the capacity and energy density of activated carbon electrodes.
