Quick-charge type negative electrode active material and preparation method thereof, negative electrode plate, secondary battery and electric device

By using the carbon-based material particles modified by cladding and ferroelectric materials in secondary batteries, the resistance problem of graphite negative electrode active materials during fast charging is solved, and the high energy density and fast charging is achieved, which extends the battery's Cycle life.

CN119092681AActive Publication Date: 2024-12-06CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411213701.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-06-24
Publication Date
2024-12-06
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

The fast charging capacity of existing secondary batteries is limited by graphite negative electrode active materials, especially when charging at large-scale, it is easy to induce lithium dendrites and dead lithium, resulting in a reduced energy density and a shortened cycle life.

Method used

Using a fast charging negative electrode active material including carbon-based material particles, a cladding layer and a ferroelectric material dispersed in the cladding layer, a conductive carbon material cladding layer is formed by carbonization sintering treatment, and at least part of the ferroelectric material is protruded. On the surface of the cladding layer, the resistance of lithium ions embedded in the negative electrode and the solid phase diffusion rate of the lithium ion embedded in the lithium ion is reduced.

Benefits of technology

It significantly improves the fast charging capability and circulation performance of the secondary battery, while maintaining high energy density, avoiding the formation of lithium dendrites and dead lithium, and extending the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092681A_ABST
    Figure CN119092681A_ABST
Patent Text Reader

Abstract

The invention provides a quick-charge type negative electrode active material and a preparation method thereof, a negative electrode plate, a secondary battery and an electric device. The fast-charging type negative electrode active material comprises carbon-based material particles, a coating layer located on at least one part of the surface of the carbon-based material particles and a ferroelectric material dispersed in the coating layer, the coating layer comprises a conductive carbon material, and at least one part of the ferroelectric material protrudes out of the surface of the coating layer. The fast charging type negative electrode active material provided by the invention has good dynamic performance, can bear high-rate charging, improves the fast charging capability of the secondary battery, and does not sacrifice the high energy density of the secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 202280005863.0, application date June 24, 2022, and invention name "Fast charging negative electrode active material and preparation method thereof, negative electrode sheet, secondary battery and electrical device". Technical Field

[0002] The present application belongs to the field of battery technology, and specifically relates to a fast-charging negative electrode active material and a preparation method thereof, a negative electrode plate, a secondary battery and an electrical device. Background Art

[0003] In recent years, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the application and promotion of secondary batteries, people have higher and higher requirements for the fast charging capacity of secondary batteries, and the negative electrode active material, as an important component of secondary batteries, has a great influence on the charging capacity of secondary batteries. At present, graphite is one of the most commonly used negative electrode active materials for secondary batteries. However, the fast charging capacity of conventional graphite has reached a bottleneck and cannot meet people's requirements for higher fast charging capacity of secondary batteries. Summary of the invention

[0004] The purpose of the present application is to provide a fast-charging negative electrode active material and a preparation method thereof, a negative electrode plate, a secondary battery and an electrical device, which can enable the secondary battery to have a significantly improved fast charging capability while having a high energy density.

[0005] The first aspect of the present application provides a fast-charging negative electrode active material, wherein the fast-charging negative electrode active material includes carbon-based material particles, a coating layer located on at least a portion of the surface of the carbon-based material particles, and a ferroelectric material dispersed in the coating layer, the coating layer includes a conductive carbon material, and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0006] The negative electrode active material of the present application can reduce the kinetic energy barrier of the desolvation process, accelerate the speed of lithium ions reaching the surface of carbon-based material particles, and reduce the resistance of lithium ions to embed into the negative electrode under the premise of containing less inactive components; the negative electrode active material of the present application can also increase the rate of solid phase diffusion of lithium embedded products from the particle surface to the interior. Therefore, the negative electrode active material of the present application has good kinetic properties, can withstand high-rate charging, and improve the fast charging capability of the secondary battery without sacrificing the high energy density of the secondary battery.

[0007] In any embodiment of the present application, the average thickness of the coating layer is H nm, the volume average particle size Dv50 of the ferroelectric material is d1 nm, and the fast-charging type negative electrode active material satisfies: 0.25 ≤ H / d1 ≤ 1.1. Optionally, 0.25 ≤ H / d1 ≤ 0.5. This is beneficial for the secondary battery to have high fast-charging ability, high energy density, and good cycling performance simultaneously.

[0008] In any embodiment of the present application, the volume average particle size Dv50 of the ferroelectric material is d1 nm, where 0 < d1 ≤ 200. Optionally, 0 < d1 ≤ 100. Thus, less ferroelectric material can be used at the same specific surface area, thereby reducing the energy density loss of the secondary battery.

[0009] In any embodiment of the present application, the average thickness of the coating layer is H nm, where 20 ≤ H ≤ 100. Optionally, 20 ≤ H ≤ 50. Thus, the secondary battery can have high fast-charging ability, high energy density, and high cycle capacity retention rate simultaneously.

[0010] In any embodiment of the present application, the mass ratio of the ferroelectric material to the carbon-based material particles is α1, and α1 is (0.5 - 10):100. Optionally, it is (1 - 3):100. This is beneficial for the secondary battery to have high fast-charging ability and high energy density simultaneously.

[0011] In any embodiment of the present application, the mass ratio of the coating layer to the carbon-based material particles is α2, and α2 is (2 - 10):100. Optionally, it is (2 - 5):100. This is beneficial for the negative electrode active material to have high fast-charging ability while also having high specific capacity, high first Coulomb efficiency, and high tap density.

[0012] In any embodiment of the present application, the mass ratio of the ferroelectric material to the carbon-based material particles is α1, and the mass ratio of the coating layer to the carbon-based material particles is α2. The ratio of α1:α2 is from 1:6 to 4:1. Optionally, it is from 1:4 to 2:1. This is beneficial for the secondary battery to have high fast-charging ability, high energy density, and high cycle capacity retention rate simultaneously.

[0013] In any embodiment of the present application, the graphitization degree of the coating layer is 45% to 80%.

[0014] In any embodiment of the present application, the conductive carbon material in the coating layer includes amorphous carbon. Optionally, it includes hard carbon. This can further improve the fast-charging ability of the secondary battery.

[0015] In any embodiment of the present application, the graphitization degree of the carbon-based material particles is 88% to 96%.

[0016] In any embodiment of the present application, the volume average particle size Dv50 of the carbon-based material particles is d2 μm, 5≤d2≤20, and optionally, 8≤d2≤15. This enables the secondary battery to have a higher rapid charging capability.

[0017] In any embodiment of the present application, the carbon-based material particles are in the form of primary particles, secondary particles or a combination thereof, and optionally, in the carbon-based material particles in the form of secondary particles, the ratio of the volume average particle size Dv50 of the primary particles to the volume average particle size Dv50 of the secondary particles they form is 0.2 to 0.5. This is beneficial for the carbon-based material particles to have good ion transport and electron transport properties while also having high structural stability.

[0018] In any embodiment of the present application, the carbon-based material particles include one or more selected from graphite, mesocarbon microspheres, hard carbon and soft carbon, and are optionally selected from graphite, thereby enabling the secondary battery to have high energy density and high cycle stability.

[0019] In any embodiment of the present application, the dielectric constant of the ferroelectric material is greater than 100, and optionally is 100 to 100000. This can better reduce the kinetic energy barrier of the desolvation process and improve the fast charging capability of the secondary battery.

[0020] In any embodiment of the present application, the Curie temperature of the ferroelectric material is above 80° C. This can better reduce the kinetic energy barrier of the desolvation process and improve the fast charging capability of the secondary battery.

[0021] In any embodiment of the present application, the ferroelectric material includes a combination of one or more selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate and lithium tantalate.

[0022] In any embodiment of the present application, the volume average particle size Dv50 of the fast-charging negative electrode active material is 5 μm to 20 μm, and optionally 8 μm to 15 μm, which is beneficial for the negative electrode active material to have better ion transport and electron transport performance and fast charging performance.

[0023] In any embodiment of the present application, the specific surface area of ​​the fast-charging negative electrode active material is 0.8 m 2 / g to 1.3m 2 / g, optionally 0.9m 2 / g to 1.2m 2 / g. This enables the secondary battery to have a higher rapid charging capability.

[0024] In any embodiment of the present application, the powder compaction density of the fast-charging negative electrode active material under a force of 20000N is 1.5g / cm 3 Up to 1.9g / cm 3 , optionally 1.5 g / cm 3 Up to 1.7g / cm 3 This enables the secondary battery to have a higher energy density and improved cycle performance.

[0025] The second aspect of the present application provides a method for preparing a fast-charging negative electrode active material, comprising the steps of: S10, providing carbon-based material particles, a carbon source and a ferroelectric material, optionally, the carbon source comprises a combination of one or more selected from asphalt, resin, and biomass materials; S20, uniformly mixing the carbon-based material particles, the carbon source and the ferroelectric material, and forming a coating layer comprising a conductive carbon material on at least a portion of the surface of the carbon-based material particles through carbonization and sintering, wherein the ferroelectric material is dispersed in the coating layer and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0026] In any embodiment of the present application, the carbonization sintering temperature in S20 is 700°C to 1800°C, and optionally 1000°C to 1300°C.

[0027] In any embodiment of the present application, the carbonization sintering time in S20 is 1 h to 15 h, optionally 6 h to 14 h.

[0028] In any embodiment of the present application, the carbon-based material particles are prepared by the following method: S101, providing coke powder, and placing the coke powder in a reaction container; S102, graphitizing the coke powder to obtain carbon-based material particles.

[0029] The third aspect of the present application provides a negative electrode plate, including a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes the fast-charging negative electrode active material of the first aspect of the present application or the fast-charging negative electrode active material prepared by the method of the second aspect of the present application.

[0030] A fourth aspect of the present application provides a secondary battery, comprising the negative electrode plate of the third aspect of the present application.

[0031] A fifth aspect of the present application provides an electrical device, comprising the secondary battery of the fourth aspect of the present application.

[0032] The fast-charge type negative electrode active material provided in the present application has good kinetic properties, can withstand high-rate charging, and improves the fast charging capability of the secondary battery without sacrificing the high energy density of the secondary battery. The electric device of the present application includes the secondary battery provided in the present application, and thus has at least the same advantages as the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some implementation methods of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.

[0034] Figure 1 It is a schematic diagram of an embodiment of the fast-charging negative electrode active material of the present application.

[0035] Figure 2 It is a schematic diagram of one embodiment of the secondary battery of the present application.

[0036] Figure 3 yes Figure 2 An exploded schematic diagram of an embodiment of a secondary battery.

[0037] Figure 4 It is a schematic diagram of an embodiment of a battery module of the present application.

[0038] Figure 5 It is a schematic diagram of an embodiment of the battery pack of the present application.

[0039] Figure 6 yes Figure 5 An exploded schematic diagram of an embodiment of a battery pack is shown.

[0040] Figure 7 It is a schematic diagram of one embodiment of an electric device including the secondary battery of the present application as a power source.

[0041] In the drawings, the drawings may not be drawn according to the actual scale. The reference numerals are as follows: 1 battery pack, 2 upper box, 3 lower box, 4 battery module, 5 secondary battery, 51 shell, 52 electrode assembly, 53 cover plate, 10 fast-charging negative electrode active material, 101 carbon-based material particles, 102 coating layer, 103 ferroelectric material. DETAILED DESCRIPTION

[0042] Below, the fast-charging negative electrode active material and its preparation method, negative electrode plate, secondary battery and electric device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0043] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0044] If not otherwise specified, all embodiments and optional embodiments of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0045] Unless otherwise specified, all technical features and optional technical features of the present application may be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of the present application.

[0046] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0047] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0048] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0049] In the present application, the terms "plurality" and "multiple" refer to two or more.

[0050] In the present application, "about" a numerical value indicates a range, which means a range of ±10% of the numerical value.

[0051] The key to improving the fast charging capability of secondary batteries lies in improving the performance of negative electrode active materials and negative electrode sheets. In the charging process of secondary batteries, taking graphite as an example, the electrode kinetics process usually includes the following steps. (1) Liquid phase mass transfer step in the electrolyte phase: the solvated lithium ions in the electrolyte diffuse and transfer to the surface of graphite particles; (2) Surface conversion step: during the first charge, the solvated lithium ions are adsorbed on the surface of the graphite particles to react and form a solid electrolyte interface (SEI) film. During the subsequent charging process, the solvated lithium ions are adsorbed on the surface of the SEI film. After the desolvation process, the lithium ions reach the surface of the graphite particles; (3) Charge exchange step: lithium ions obtain electrons from the surface of the graphite particles and form lithium intercalation products; (4) Solid phase mass transfer step of lithium intercalation products: the lithium intercalation products diffuse from the surface of the graphite particles to the interior to complete the charging process.

[0052] Existing studies generally believe that the solid-phase diffusion rate of lithium-intercalated products is slow, so the above step (4) is considered to be the control step of the negative electrode kinetic process. Therefore, existing studies mainly focus on how to increase the solid-phase diffusion rate of lithium-intercalated products and shorten the solid-phase diffusion distance. For example, in order to improve the fast charging ability of graphite, the methods used in the existing technology mainly include: (1) etching pores on the graphite surface to increase the surface active sites and lithium ion embedding channels, thereby shortening the lithium ion diffusion distance; (2) coating graphite with amorphous carbon to increase the interlayer spacing of the graphite surface and increase the diffusion rate of lithium ions. However, the above methods have limited effect on improving the fast charging ability of secondary batteries.

[0053] The inventors of this application have studied the electrode kinetics during charging of secondary batteries in detail and found that an important factor affecting the improvement of graphite's fast charging ability is the influence of the electrolyte solvation. The electrolyte is usually obtained by uniformly mixing lithium salts and solvent molecules, so that the electrolyte usually includes three components: solvent molecules, anions, and solvated lithium ions. Before the lithium ions reach the surface of the graphite particles and embed into the graphite particles during the charging process, the solvated lithium ions need to undergo a desolvation process to remove the solvent molecules, but this process has a high kinetic energy barrier, for example, about 50kJ / mol to 70kJ / mol.

[0054] In addition, the generation of "lithium dendrites" and "dead lithium" is another important factor that affects the improvement of the fast charging ability of secondary batteries. During the charging process of secondary batteries, when the negative electrode has insufficient lithium embedding space, the resistance of lithium ions embedding into the negative electrode is too large, the lithium ions are too quickly released from the positive electrode but cannot be embedded in the negative electrode in equal amounts, the lithium ions that cannot be embedded in the negative electrode can only obtain electrons on the surface of the negative electrode, thus forming a silvery-white metallic lithium single substance, namely "lithium dendrites". The formation of lithium dendrites not only reduces the performance of secondary batteries, such as shortening the cycle life, but also forms a sharp morphology that pierces the isolation membrane and causes a short circuit in the battery in severe cases, which may cause catastrophic consequences such as combustion and explosion. At the same time, the continuously deposited metallic lithium single substance will also fall off from the surface of the negative electrode, thereby forming "dead lithium" that can no longer participate in the reaction, resulting in a decrease in the energy density of the secondary battery.

[0055] The inventors of the present application also found in the process of studying the electrode kinetics during charging of secondary batteries that due to the presence of a high kinetic energy barrier in the desolvation process, the speed at which lithium ions reach the surface of graphite particles is limited, thereby increasing the resistance to lithium ion embedding into the negative electrode. In particular, when the secondary battery is rapidly charged at a high rate, it is more likely to induce "lithium dendrites" and "dead lithium".

[0056] After extensive research, the inventors of the present application have proposed a new type of fast-charging negative electrode active material, which can enable secondary batteries to have a significantly improved fast charging capability while having a high energy density. Negative electrode active material

[0057] Specifically, a first aspect of the embodiments of the present application provides a fast-charging negative electrode active material.

[0058] The fast-charging negative electrode active material includes carbon-based material particles, a coating layer located on at least a portion of the surface of the carbon-based material particles, and a ferroelectric material dispersed in the coating layer. The coating layer includes a conductive carbon material, and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0059] The negative electrode active material of the present application has good kinetic properties and can improve the fast charging capability of the secondary battery without sacrificing the high energy density of the secondary battery. Although the mechanism is not clear, the inventor speculates that the possible reasons include the following points.

[0060] First, the surface of the negative electrode active material of the present application has a ferroelectric material, which has a spontaneous polarization strength, and the spontaneous polarization strength can be reversed when the external electric field is reversed, thereby reducing the kinetic energy barrier of the desolvation process of the solvated lithium ions, accelerating the speed at which the lithium ions reach the surface of the carbon-based material particles, and reducing the resistance of the lithium ions to be embedded in the negative electrode. Therefore, the negative electrode active material of the present application has good kinetic properties and can withstand high-rate charging, thereby improving the fast charging capability of the secondary battery.

[0061] Second, in the negative electrode active material of the present application, at least part of the ferroelectric material protrudes from the surface of the coating layer, so that the part of the ferroelectric material can directly contact both the electrolyte and the carbon-based material particles. The surface of the ferroelectric material in contact with the electrolyte is induced to be negatively charged, and the surface of the ferroelectric material in contact with the carbon-based material particles is induced to be positively charged, thereby better reducing the kinetic energy barrier of the desolvation process, accelerating the speed at which lithium ions reach the surface of the carbon-based material particles, and reducing the resistance of lithium ions to embed into the negative electrode. Therefore, the negative electrode active material of the present application has good kinetic properties and can withstand high-rate charging, thereby improving the fast charging capability of the secondary battery.

[0062] Third, as the charging process proceeds, the amount of lithium embedded in the negative electrode gradually increases, and the activation energy that needs to be overcome when the lithium embedded product diffuses from the particle surface to the interior increases, making solid phase diffusion more difficult. In the negative electrode active material of the present application, the coating layer includes a conductive carbon material with good conductivity, thereby increasing the rate of solid phase diffusion of the lithium embedded product from the particle surface to the interior, so that the negative electrode active material has good kinetic properties.

[0063] Fourth, in the negative electrode active material of the present application, the conductive carbon material and the carbon-based material particles in the coating layer are both active components and can contribute to capacity, while the ferroelectric material is an inactive component and cannot contribute to capacity, but can reduce the kinetic energy barrier of the desolvation process, accelerate the speed at which lithium ions reach the surface of the carbon-based material particles, and reduce the resistance of lithium ions to embed into the negative electrode. The negative electrode active material of the present application disperses the ferroelectric material in the coating layer, and also makes at least part of the ferroelectric material protrude from the surface of the coating layer, so that the ferroelectric material has a larger exposed surface area and a larger contact area with the electrolyte, thereby being able to achieve the effect of reducing the kinetic energy barrier of the desolvation process when the dosage is small. Therefore, the secondary battery using the negative electrode active material of the present application has a high fast charging capability while not sacrificing high energy density.

[0064] The negative electrode active material of the present application can reduce the kinetic energy barrier of the desolvation process, accelerate the speed of lithium ions reaching the surface of carbon-based material particles, and reduce the resistance of lithium ions to embed into the negative electrode under the premise of containing less inactive components; the negative electrode active material of the present application can also increase the rate of solid phase diffusion of lithium embedded products from the particle surface to the interior. Therefore, the negative electrode active material of the present application has good kinetic properties, can withstand high-rate charging, and improve the fast charging capability of the secondary battery without sacrificing the high energy density of the secondary battery.

[0065] In some embodiments, optionally, all ferroelectric materials protrude from the surface of the coating layer, thereby exposing more surface area of ​​the ferroelectric material and increasing the contact area with the electrolyte, thereby being able to achieve the effect of reducing the kinetic energy barrier of the desolvation process when using less amount.

[0066] In some embodiments, the average thickness of the coating layer is H nm, the volume average particle size Dv50 of the ferroelectric material is d1 nm, and the fast-charging type negative electrode active material satisfies: 0.25 ≤ H / d1 ≤ 1.1. When H / d1 is less than 1.1, at least part of the ferroelectric material can protrude from the surface of the coating layer, thereby increasing the contact area with the electrolyte, so that the kinetic energy barrier of the desolvation process can be reduced with less dosage. When H / d1 is less than 0.25, the contact area between the ferroelectric material and the electrolyte is large, and the kinetic energy barrier of the desolvation process can be better reduced. However, at this time, the overall negative electrode active material is not easily compacted, resulting in possible deterioration of the ionic conduction ability and electronic conduction ability of the negative electrode sheet, which may in turn affect the fast charging ability, energy density and cycle performance of the secondary battery. Therefore, when H / d1 is within a suitable range, it is beneficial for the secondary battery to have high fast charging ability, high energy density and good cycle performance. Optionally, 0.25 ≤ H / d1 ≤ 1.0, 0.25 ≤ H / d1 ≤ 0.9, 0.25 ≤ H / d1 ≤ 0.8, 0.25 ≤ H / d1 ≤ 0.7, 0.25 ≤ H / d1 ≤ 0.6, 0.25 ≤ H / d1 ≤ 0.5, 0.25 ≤ H / d1 ≤ 0.4, 0.30 ≤ H / d1 ≤ 0.9, 0.30 ≤ H / d1 ≤ 0.8, 0.30 ≤ H / d1 ≤ 0.7, 0.30 ≤ H / d1 ≤ 0.6, 0.30 ≤ H / d1 ≤ 0.5, 0.30 ≤ H / d1 ≤ 0.4, 0.35 ≤ H / d1 ≤ 0.9, 0.35 ≤ H / d1 ≤ 0.8, 0.35 ≤ H / d1 ≤ 0.7, 0.35 ≤ H / d1 ≤ 0.6 or 0.35 ≤ H / d1 ≤ 0.5.

[0067] In some embodiments, the volume average particle size Dv50 of the ferroelectric material is d1 nm, and 0 < d1 ≤ 200. Optionally, 0 < d1 ≤ 180, 0 < d1 ≤ 160, 0 < d1 ≤ 140, 0 < d1 ≤ 120, 0 < d1 ≤ 100, 0 < d1 ≤ 80, 0 < d1 ≤ 60, 0 < d1 ≤ 40, 20 ≤ d1 ≤ 180, 20 ≤ d1 ≤ 160, 20 ≤ d1 ≤ 140, 20 ≤ d1 ≤ 120, 20 ≤ d1 ≤ 100, 20 ≤ d1 ≤ 80, 20 ≤ d1 ≤ 60, 20 ≤ d1 ≤ 40, 30 ≤ d1 ≤ 180, 30 ≤ d1 ≤ 160, 30 ≤ d1 ≤ 140, 30 ≤ d1 ≤ 120, 30 ≤ d1 ≤ 100, 30 ≤ d1 ≤ 80 or 30 ≤ d1 ≤ 60. The smaller the volume average particle size Dv50 of the ferroelectric material, the larger its specific surface area. Therefore, less ferroelectric material can be used at the same specific surface area, thereby reducing the energy density loss of the secondary battery.

[0068] In some embodiments, the average thickness of the coating layer is H nm, 20≤H≤100. The coating layer includes a conductive carbon material with good conductivity, thereby increasing the rate of solid-phase diffusion of lithium-inserted products from the particle surface to the interior, so that the negative electrode active material has good kinetic properties. Therefore, when the thickness of the coating layer is thicker, the fast charging capability of the secondary battery can be improved, but the conductive carbon material in the coating layer has more pores, more surface defects and a larger specific surface area. Therefore, when the thickness of the coating layer is thicker, there are more interfacial side reactions between the negative electrode active material and the electrolyte, which easily leads to a low first coulomb efficiency and a faster capacity decay of the negative electrode active material. Therefore, when the average thickness of the coating layer is within a suitable range, it is beneficial for the negative electrode active material to have a high fast charging capability while also having a high gram capacity and a high first coulomb efficiency, so that the secondary battery can simultaneously have a high fast charging capability, a high energy density and a high cycle capacity retention rate. Optionally, 20≤H≤95, 20≤H≤90, 20≤H≤85, 20≤H≤80, 20≤H≤75, 20≤H≤70, 20≤H≤65, 20≤H≤60, 20≤H≤55, 20≤H≤50, 20≤H≤45 or 20≤H≤40.

[0069] In some embodiments, optionally, the dielectric constant of the ferroelectric material is greater than 100. When the ferroelectric material has a high dielectric constant, its surface can provide a new path for the desolvation process of the solvated lithium ions, and the higher the dielectric constant of the ferroelectric material, the better the effect of reducing the kinetic energy barrier of the desolvation process, but its effect will not continue to increase. At the same time, the higher the dielectric constant, the higher the requirements for the preparation process of the ferroelectric material, thereby increasing the production cost. In some embodiments, optionally, the dielectric constant of the ferroelectric material can be 100 to 100000, for example, it can be 100 to 50000, 100 to 25000, 100 to 10000, 100 to 5000, 100 to 4000, 100 to 3000, 100 to 2000, 100 to 1000, 100 to 500, 150 to 50000, 150 to 25 000, 150 to 10,000, 150 to 5,000, 150 to 4,000, 150 to 3,000, 150 to 2,000, 150 to 1,000, 150 to 500, 200 to 50,000, 200 to 25,000, 200 to 10,000, 200 to 5,000, 200 to 4,000, 200 to 3,000, 200 to 2,000 or 200 to 1,000.

[0070] In the present application, the dielectric constant of ferroelectric material refers to the dielectric constant at room temperature (25±5°C), which has a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, the ferroelectric material can be prepared into a circular sample, and the capacitance C can be tested using an LCR tester and calculated according to the formula: dielectric constant ε = (C×d) / (ε0×A). C represents capacitance, in farads (F); d represents sample thickness, in cm; A represents sample area, in cm 2 ; ε0 represents the dielectric constant of vacuum, ε0=8.854×10 -14 F / cm. In this application, the test conditions may be 1KHz, 1.0V, 25±5°C. The test standard may be based on GB / T 11297.11-2015. When preparing the sample, reference may be made to Chinese patent application CN114217139A.

[0071] In some embodiments, optionally, the dielectric constant of the ferroelectric material is higher than the dielectric constant of the electrolyte, thereby being able to better reduce the kinetic energy barrier of the desolvation process and improve the fast charging capability of the secondary battery.

[0072] In some embodiments, the ferroelectric material is insoluble in water and has a relatively high Curie temperature, for example, generally above 80° C. Thus, the ferroelectric material can be better utilized during the use of the secondary battery.

[0073] In some embodiments, optionally, the ferroelectric material comprises a combination of one or more selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate (LiNbO3) and lithium tantalate (LiTaO3). More optionally, the ferroelectric material is selected from perovskite structure oxides.

[0074] Optionally, the perovskite structure oxide has a molecular formula of Ba 1-x A x Ti 1-y B y O3. A includes one or more selected from the group consisting of Pb, Sr, Ca, K, Na and Cd, B includes one or more selected from the group consisting of Sn, Hf, Zr, Ce, Nb and Th, 0≤x≤1, 0≤y≤1. For example, the perovskite structure oxide may include one or more selected from the group consisting of BaTiO3, Ba 1-x1 Sr x1 TiO3(0≤x1≤1), SrTiO3, PbTiO3, PbZr y1 Ti 1-y1 O3(0≤y1≤1), BaZr y2 Ti 1-y2One or a combination of more of O3 (0 < y2 < 1), KNbO3, and NaNbO3.

[0075] Optionally, the tungsten bronze type compound may have the molecular formula M z WO3. M includes a combination of one or more selected from Na, K, Rb, and Cs, and 0 < z < 1. For example, the tungsten bronze type compound may include one or a combination of more selected from Na z1 WO3 (0 < z1 < 1), K z2 WO3 (0 < z2 < 1).

[0076] Optionally, the bismuth oxide type layered structure compound has the molecular formula (Bi2O2)(C n-1 D n O 3n+1 ). C includes a combination of one or more selected from Na, K, Ba, Sr, Pb, Ca, Ln, and Bi, D includes a combination of one or more selected from Zr, Cr, Nb, Ta, Mo, W, Fe, Ti, and V, and 2 ≤ n ≤ 5. For example, the bismuth oxide type layered structure compound may be one or a combination of more of SrBi2Nb2O9, SrBi2Ta2O9, SrBi2Nb2O9, Bi4Ti3O 12 .

[0077] In some embodiments, the mass ratio of the ferroelectric material to the carbon-based material particles is α1, and α1 is (0.5 - 10):100. Optionally, α1 is (0.5 - 9):100, (0.5 - 8):100, (0.5 - 7):100, (0.5 - 6):100, (0.5 - 5):100, (0.5 - 4):100, (0.5 - 3):100, (1 - 9):100, (1 - 8):100, (1 - 7):100, (1 - 6):100, (1 - 5):100, (1 - 4):100, or (1 - 3):100.

[0078] When α1 is within a suitable range, it is beneficial for the secondary battery to have both high fast charging ability and high energy density. And it can also effectively avoid the following situations: when α1 is larger, the content of non-active components in the negative electrode active material particles increases, and the content of active components decreases, which may cause the secondary battery to lose more energy density; when α1 is larger, the ferroelectric material may also cover more surfaces of the negative electrode active material, thereby reducing the active sites on the surface of the negative electrode active material, which may also lead to a deterioration in the fast charging ability and cycling performance of the secondary battery; when α1 is smaller, the content of the ferroelectric material is less, and its effect of reducing the kinetic energy barrier of the desolvation process may not be obvious, which may be disadvantageous for improving the fast charging ability of the secondary battery.

[0079] In some embodiments, the mass ratio of the coating layer to the carbon-based material particles is α2, and α2 is (2-10): 100. Optionally, α2 is (2-9): 100, (2-8): 100, (2-7): 100, (2-6): 100, (2-5): 100, (3-9): 100, (3-8): 100, (3-7): 100, (3-6): 100 or (3-5): 100.

[0080] When α2 is within a suitable range, it is beneficial for the negative electrode active material to have high fast charging capability while also having high gram capacity, high first coulomb efficiency and high compaction density, so that the secondary battery can have high fast charging capability, high energy density and high cycle capacity retention rate at the same time. And it can also effectively avoid the following situations: when α2 is large, the coating layer is thicker and the content of the conductive carbon material is higher. Since the conductive carbon material has more pores and a larger specific surface area, there are more interface side reactions between the negative electrode active material and the electrolyte; at the same time, when α2 is large, the surface morphology of the conductive carbon material is rough and there are more surface defects, which makes it difficult for the negative electrode active material to be compacted. In addition, due to the unstable surface defect structure of the conductive carbon material, it is also easy to cause the first coulomb efficiency of the negative electrode active material to be low and the capacity decay to be fast, which may also make the capacity performance and cycle performance of the secondary battery worse; when α2 is small, it is not conducive to the rapid insertion and extraction of lithium ions, which may be unfavorable to improve the rapid charging capability of the secondary battery.

[0081] In some embodiments, the mass ratio of the ferroelectric material to the carbon-based material particles is α1, the mass ratio of the coating layer to the carbon-based material particles is α2, and α1:α2 is 1:6 to 4:1, and optionally 1:4 to 2:1.

[0082] When α1:α2 is within a suitable range, it is beneficial for the negative electrode active material to have high fast charging capability while also having high gram capacity, high first coulomb efficiency and high compaction density, so that the secondary battery can have high fast charging capability, high energy density and high cycle capacity retention rate at the same time. And it can also effectively avoid the following situations: when α1:α2 is large, the content of inactive components in the negative electrode active material particles increases and the content of active components decreases, which may cause the secondary battery to lose more energy density and is not conducive to the rapid insertion and extraction of lithium ions; when α1:α2 is small, the content of ferroelectric materials is small, and its role in reducing the kinetic energy barrier of the desolvation process may not be obvious, which may deteriorate the fast charging capability of the secondary battery and easily lead to low first coulomb efficiency and rapid capacity decay of the negative electrode active material.

[0083] The coating layer includes a conductive carbon material. Optionally, the conductive carbon material includes amorphous carbon. Amorphous carbon refers to a transitional carbon material with a low degree of graphitization crystallization and an approximately amorphous form (or no fixed shape and periodic structural regularity), which can be obtained by carbonization and sintering of a carbon source (such as asphalt, resin, biomass material, etc.). The interlayer spacing of amorphous carbon is large, and it does not cause volume shrinkage and expansion effects during the extraction and embedding of lithium ions, so that its crystal structure is more stable, which can make the negative electrode active material have good kinetic properties and withstand high-rate charging, thereby improving the fast charging capability of the secondary battery. The amorphous carbon includes soft carbon, hard carbon or a combination thereof. Optionally, in some embodiments, the conductive carbon material includes hard carbon, thereby further improving the fast charging capability of the secondary battery.

[0084] In some embodiments, the carbon-based material particles include one or more combinations selected from graphite (e.g., artificial graphite, natural graphite, graphite oxide, etc.), mesophase carbon microspheres, hard carbon and soft carbon, optionally selected from graphite. Graphite has the advantages of stable cycle performance and high gram capacity, thereby enabling the secondary battery to have high energy density and high cycle stability.

[0085] In some embodiments, the coating layer has a graphitization degree of 45% to 80%.

[0086] In some embodiments, the carbon-based material particles have a degree of graphitization of 88% to 96%.

[0087] The inventors have found that when the coating layer and the carbon-based material particles also meet the graphitization degree within the above range, it helps to reasonably match the crystal structure of the coating layer and the carbon-based material particles, thereby effectively improving the solid-phase diffusion rate of lithium ions, thereby improving the rapid charging capability and cycle performance of the secondary battery.

[0088] In some embodiments, the morphology of the carbon-based material particles is primary particles, secondary particles or a combination thereof. Secondary particles are generally obtained by agglomeration of primary particles. Optionally, in the carbon-based material particles with the secondary particle morphology, the ratio of the volume average particle size Dv50 of the primary particles to the volume average particle size Dv50 of the secondary particles they constitute is 0.2 to 0.5. When the carbon-based material particles are in the morphology of secondary particles and the ratio of the volume average particle size Dv50 of the primary particles to the volume average particle size Dv50 of the secondary particles they constitute is adjusted within a suitable range, it is beneficial for the carbon-based material particles to have a good degree of secondary particles, so that they can have good ion transport and electron transport properties while also having high structural stability.

[0089] In some embodiments, the volume average particle size Dv50 of the carbon-based material particles is d2 μm, 5≤d2≤20, optionally, 8≤d2≤15. When the volume average particle size Dv50 of the carbon-based material particles is within a suitable range, it is beneficial for the negative electrode active material of the present application to have a higher electrochemical activity, thereby enabling the secondary battery to have a higher fast charging capability. And it can also effectively avoid the following situations: when the volume average particle size Dv50 of the carbon-based material particles is small, the gram capacity of the negative electrode active material is low and the compaction density is low, which is not conducive to the design of high energy density batteries; at the same time, when the volume average particle size Dv50 of the carbon-based material particles is small, its specific surface area is large and the reaction activity is high, which may increase the interfacial side reactions between the negative electrode active material and the electrolyte, and then lead to an increase in the irreversible consumption of active lithium ions, and the capacity and energy density of the secondary battery may deteriorate; when the volume average particle size Dv50 of the carbon-based material particles is large, the active sites on the particle surface are reduced, and the path for the lithium-embedded product to diffuse from the solid phase of the particle surface to the interior is longer, which may be not conducive to the improvement of the fast charging capability of the secondary battery.

[0090] In some embodiments, the volume average particle size Dv50 of the fast-charging negative electrode active material is 5 μm to 20 μm, and optionally 8 μm to 15 μm. By adjusting the volume average particle size Dv50 of the negative electrode active material within a suitable range, the negative electrode active material is beneficial to having better ion transport and electron transport performance and fast charging performance, while also having a higher powder compaction density.

[0091] In some embodiments, the specific surface area of ​​the fast-charging negative electrode active material is 0.8 m 2 / g to 1.3m 2 / g, optionally 0.9m 2 / g to 1.2m 2 By adjusting the specific surface area of ​​the negative electrode active material within a suitable range, the interface side reaction between the negative electrode plate and the electrolyte can be reduced, and the negative electrode plate can have a suitable electrochemical reaction activity, thereby enabling the secondary battery to have a higher rapid charging capability.

[0092] In some embodiments, the powder compaction density of the fast-charging negative electrode active material under a force of 20,000 N is 1.5 g / cm 3 Up to 1.9g / cm 3 , optionally 1.5 g / cm 3 Up to 1.7g / cm 3By adjusting the compaction density of the negative electrode active material powder within a suitable range, the negative electrode film layer can have a higher compaction density, and thus the secondary battery has a higher energy density. In addition, by adjusting the compaction density of the negative electrode active material powder within a suitable range, the negative electrode film layer can also have a stronger ability to maintain the pore structure during the cycle, thereby improving the electrolyte wettability of the negative electrode plate and better improving the cycle performance of the secondary battery.

[0093] In the present application, the average thickness of the coating layer has a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, a transmission electron microscope can be used to obtain a TEM (Transmission Electron Microscope) image, and then the thickness of multiple (for example, more than 30) different positions on the TEM image can be measured, and the average value is taken as the average thickness of the coating layer.

[0094] In this application, the volume average particle size Dv50 of the material has a well-known meaning in the art, which indicates the particle size corresponding to when the cumulative volume distribution percentage of the material reaches 50%, and can be tested using instruments and methods known in the art. For example, it can be conveniently tested using a laser particle size analyzer with reference to GB / T 19077-2016 particle size distribution laser diffraction method, such as the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK.

[0095] In this application, the graphitization degree of a material is a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, an X-ray diffractometer (such as Bruker D8 Discover) can be used for testing. The test can refer to JIS K 0131-1996 and JB / T 4220-2011 to obtain d 002 Then according to the formula g = (0.344-d 002 ) / (0.344-0.3354)×100% to calculate the graphitization degree of the material. In the above formula, d 002 It is the interlayer spacing of the (002) crystal plane in the material's crystal structure expressed in nanometers (nm).

[0096] In this application, the specific surface area of ​​a material is a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, it can be tested by nitrogen adsorption specific surface area analysis test method according to GB / T 19587-2017 and calculated using the BET (BrunauerEmmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed using the Tri-Star 3020 specific surface area pore size analysis tester from Micromeritics, USA.

[0097] In this application, the powder compaction density of a material has a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, it can be tested by an electronic pressure testing machine (such as UTM7305) with reference to the standard GB / T24533-2009. An exemplary test method is as follows: weigh 1g of material and add a bottom area of ​​1.327cm 2 The mold is pressurized to 2000kg (equivalent to 20000N), maintained for 30s, then released, maintained for 10s, and then the powder compaction density of the material under a force of 20000N is recorded and calculated.

[0098] It should be noted that the above-mentioned various parameter tests for the negative electrode active material can be sampled and tested before coating, or can be sampled and tested from the negative electrode film layer after cold pressing. When the negative electrode active material test sample is sampled from the negative electrode film layer after cold pressing, as an example, the sampling can be carried out according to the following steps: arbitrarily select a cold pressed negative electrode film layer and sample the negative electrode active material (for example, a blade can be used to scrape the powder for sampling); place the above collected negative electrode active material powder in deionized water, then filter and dry it, and then sinter the dried negative electrode active material at a certain temperature and time (for example, 400°C, 2h), remove the binder and the conductive agent, and obtain the negative electrode active material test sample.

[0099] The fast-charging negative electrode active material of the present application is described below with reference to the accompanying drawings. Figure 1 Schematic diagram of an embodiment of the fast-charging negative electrode active material 10 of the present application. Figure 1 As shown, the fast-charging negative electrode active material 10 includes a carbon-based material particle 101, a coating layer 102 located on at least a portion of the surface of the carbon-based material particle 101, and a ferroelectric material 103 dispersed in the coating layer 102. The coating layer 102 includes a conductive carbon material, and at least a portion of the ferroelectric material 103 protrudes from the surface of the coating layer 102. Preparation method

[0100] The second aspect of the embodiment of the present application provides a method for preparing the fast-charging negative electrode active material of the first aspect of the present application, which includes the steps of: S10, providing carbon-based material particles, a carbon source and a ferroelectric material; S20, uniformly mixing the carbon-based material particles, the carbon source and the ferroelectric material, and forming a coating layer including a conductive carbon material on at least a portion of the surface of the carbon-based material particles through carbonization and sintering, wherein the ferroelectric material is dispersed in the coating layer and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0101] In the present application, "carbon source" refers to a compound that can form a conductive carbon material. The carbon source includes a combination of one or more selected from organic carbon sources and inorganic carbon sources. Optionally, the carbon source is an organic carbon source.

[0102] In some embodiments, optionally, the carbon source includes a combination of one or more selected from asphalt, resin, and biomass materials. As an example, the asphalt includes a combination of one or more selected from coal tar and petroleum asphalt, optionally petroleum asphalt. As an example, the resin includes a combination of one or more selected from phenolic resin and epoxy resin. As an example, the biomass material refers to a material derived from living organisms such as animals, plants and microorganisms, mainly composed of organic polymer substances, and mainly composed of three elements of carbon, hydrogen and oxygen in chemical composition, for example, it can be a polysaccharide (such as starch, sucrose polymer, glucose polymer, cellulose, etc.).

[0103] In some embodiments, optionally, the carbonization sintering temperature in S20 is 700°C to 1800°C, more optionally 1000°C to 1300°C.

[0104] In some embodiments, optionally, the carbonization sintering time in S20 is 1 h to 15 h, optionally 6 h to 14 h.

[0105] In S20, by controlling the carbonization sintering temperature and the carbonization sintering time within the above range, the carbon source can be carbonized and a coating layer containing a conductive carbon material can be formed on at least a portion of the surface of the carbon-based material particles, and the coating layer can also have a suitable thickness and degree of graphitization.

[0106] In some embodiments, the carbon-based material particles may be commercially available products, or alternatively, may be prepared by the following method: S101, providing coke powder, and placing the coke powder into a reaction container; S102, graphitizing the coke powder to obtain carbon-based material particles.

[0107] In some embodiments, the coke powder may be a commercially available product, or alternatively, may be prepared by the following method: S1011, coking the coke raw material to obtain coke; S1012, crushing, shaping, and grading the obtained coke to obtain coke powder.

[0108] In the present application, "coke raw material" refers to components that can be processed to obtain "coke", that is, raw materials for preparing coke; "coke" refers to the product obtained by coking the coke raw material; "coke powder" and "coke" are exactly the same in composition, the difference is that "coke powder" refers to "coke" in the form of powder of a certain particle size, that is, "coke powder" is obtained after "coke" is crushed and other treatments.

[0109] Optionally, the coke raw material may include a combination of one or more selected from petroleum-based raw materials and coal-based raw materials. As an example, the petroleum-based raw materials include a combination of one or more selected from heavy oil, residual oil, and vacuum residue oil, and the coal-based raw materials mainly include coal tar. Heavy oil, residual oil, and vacuum residue oil are usually produced in petroleum refining processes, and coal tar is usually produced in coal distillation processes.

[0110] Optionally, the coke obtained in S1011 includes a combination of one or more selected from petroleum non-needle coke, petroleum needle coke, coal non-needle coke, and coal needle coke. More optionally, the coke obtained in S1011 includes a combination of one or more selected from petroleum non-needle coke (e.g., petroleum calcined coke, petroleum green coke), and petroleum needle coke. In particular, the coke obtained in S1011 is petroleum green coke. The use of suitable coke can make the prepared carbon-based material particles have a suitable number of end faces and defects, and thus have better ion transport and electron transport properties and higher structural stability, thereby improving the fast charging capability and cycle performance of the secondary battery.

[0111] Optionally, the coking process of the coke raw material in S1011 is carried out in a delayed coking device. The delayed coking device includes a heating furnace and a coke drum. The delayed coking process refers to rapidly heating the coke raw material to the required coking process temperature in the heating furnace, and then entering the coke drum, and generating coke through preheating, cooling and other processes in the coke drum.

[0112] Optionally, in S1012, the obtained coke may be crushed by using equipment and methods known in the art, such as a jet mill, a mechanical mill, a roller mill or other crushing equipment.

[0113] The morphology of the coke powder obtained after crushing may include a combination of one or more of block, spherical and quasi-spherical shapes. After the crushing is completed, the coke powder is shaped to grind the edges and corners. The greater the degree of shaping, the closer the powder particles are to a sphere, which can increase the active sites on the surface of the carbon-based material particles. The shaping process is also beneficial to the subsequent granulation process, so that the secondary particle part in the obtained carbon-based material particles has a higher structural stability. The shaping process can be carried out using equipment and methods known in the art, such as a shaping machine or other shaping equipment.

[0114] During the crushing and shaping process, a large number of undersized particles and sometimes oversized particles are often produced. Therefore, classification treatment can be performed according to needs to remove undersized particles and oversized particles in the powder. After classification treatment, coke powder with a good particle size distribution can be obtained to facilitate the subsequent granulation process. Classification treatment can be carried out using equipment and methods known in the art, such as a classification screen, a gravity classifier, a centrifugal classifier, etc.

[0115] In some embodiments, optionally, S101 further includes: adding a binder to the reaction container, and granulating the binder and the coke powder after uniformly mixing them. Adding the binder can make the obtained carbon-based material particles have a good secondary particle degree, which is beneficial to improve the ion transport and electron transport performance of the negative electrode active material while making it have a higher structural stability.

[0116] Optionally, the mass percentage of the binder is 3% to 12%, more preferably 5% to 8%, based on the total mass of the coke powder. The content of the binder is within a suitable range to avoid excessive agglomeration of particles.

[0117] Optionally, the binder includes a combination of one or more selected from coal tar, petroleum asphalt, mesophase asphalt, phenolic resin, epoxy resin, and petroleum resin.

[0118] The granulation process can be carried out using equipment and methods known in the art, such as a granulator. The granulator generally includes a stirred reactor and a module for controlling the temperature of the reactor. By regulating the stirring speed, heating rate, granulation temperature, cooling rate, etc. during the granulation process, the granulation degree and the structural strength of the particles can be regulated, and the volume average particle size Dv50 of the carbon-based material particles finally prepared can be within the desired range.

[0119] In some embodiments, optionally, the graphitization treatment temperature in S102 may be 2400°C to 3200°C, more optionally 2800°C to 3200°C or 2900°C to 3100°C.

[0120] In some embodiments, optionally, the graphitization treatment time in S102 may be 20 hours to 48 hours.

[0121] Graphitization treatment can make the carbon-based material particles have a suitable degree of graphitization to increase the gram capacity of the negative electrode active material; graphitization treatment can also make the carbon-based material particles have a smaller lattice expansion rate to improve the structural stability; graphitization treatment can also effectively eliminate the bulk structural defects in the carbon-based material particles to improve the cycle stability of the secondary battery.

[0122] The graphitization treatment can be carried out using equipment and methods known in the art, such as a graphitization furnace, especially an Acheson graphitization furnace. After the graphitization treatment is completed, a small amount of oversized particles formed by agglomeration during the graphitization treatment can be removed by screening, so as to prevent the oversized particles from affecting the processing properties of the obtained negative electrode active material, such as the stability of the negative electrode slurry, coating properties, etc.

[0123] In some embodiments, the preparation method of the fast-charging negative electrode active material includes the steps of: placing coke powder and a binder into a reaction container and mixing them evenly before granulating; graphitizing the obtained granulated product to obtain carbon-based material particles; evenly mixing the obtained carbon-based material particles with a carbon source and a ferroelectric material, and forming a coating layer including a conductive carbon material on at least a portion of the surface of the carbon-based material particles through carbonization and sintering, wherein the ferroelectric material is dispersed in the coating layer and at least a portion of the ferroelectric material protrudes from the surface of the coating layer.

[0124] The preparation method of the fast-charging negative electrode active material of the present application has a simple process and low production cost, and is compatible with the current carbon-based material particles, especially the preparation process of artificial graphite, so that no additional production equipment and process steps are required. When the fast-charging negative electrode active material is prepared by the method of the present application, the ferroelectric material is not easy to agglomerate, thereby enabling the desolvation effect of the solvated lithium ions to act on the entire negative electrode active material, thereby facilitating the negative electrode active material to have a higher fast charging capability and a longer service life.

[0125] Some raw materials and their contents used in the method for preparing the fast-charging negative electrode active material of the present application can refer to the fast-charging negative electrode active material of the first aspect of the implementation method of the present application, and will not be repeated here. Negative electrode

[0126] The third aspect of the embodiment of the present application provides a negative electrode plate, the negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer includes the fast-charging negative electrode active material of the first aspect of the embodiment of the present application or the fast-charging negative electrode active material prepared by the method of the second aspect of the embodiment of the present application. For example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0127] In some embodiments, the negative electrode film layer may also include other negative electrode active materials for secondary batteries known in the art. As an example, the other negative electrode active materials include a combination of one or more selected from natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. The silicon-based material may include a combination of one or more selected from elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite and silicon alloy material. The tin-based material may include a combination of one or more selected from elemental tin, tin oxide and tin alloy material.

[0128] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application has no particular restrictions on the type of the negative electrode conductive agent. As an example, the negative electrode conductive agent may include a combination of one or more selected from superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. In some embodiments, based on the total mass of the negative electrode film layer, the mass percentage of the negative electrode conductive agent is less than 5%.

[0129] In some embodiments, the negative electrode film layer may also optionally include a negative electrode binder. The present application has no particular restrictions on the type of the negative electrode binder. As an example, the negative electrode binder may include a combination of one or more selected from styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA) and carboxymethyl chitosan (CMCS). In some embodiments, based on the total mass of the negative electrode film layer, the mass percentage of the negative electrode binder is less than 5%.

[0130] In some embodiments, the negative electrode film layer may further include other additives. As an example, other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC-Na), PTC thermistor materials, etc. In some embodiments, based on the total mass of the negative electrode film layer, the mass percentage of the other additives is less than 2%.

[0131] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, a copper foil or a copper alloy foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include a combination of one or more selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, and the polymer material base layer may include a combination of one or more selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0132] The negative electrode film layer is usually formed by coating the negative electrode slurry on the negative electrode current collector, drying and cold pressing. The negative electrode slurry is usually formed by dispersing the negative electrode active material, optional conductive agent, optional binder, and other optional auxiliary agents in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited thereto.

[0133] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate described in the present application also includes a conductive primer layer (for example, composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In some other embodiments, the negative electrode plate described in the present application also includes a protective layer covering the surface of the negative electrode film layer. Secondary battery

[0134] A fourth aspect of the embodiments of the present application provides a secondary battery, which includes the negative electrode plate according to the third aspect of the present application.

[0135] A secondary battery, also known as a rechargeable battery or storage battery, refers to a battery that can be used continuously by activating the active material by charging after the battery is discharged. A secondary battery includes an electrode assembly and an electrolyte, and the electrode assembly generally includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and mainly serves to prevent the positive and negative electrodes from short-circuiting, while allowing lithium ions to pass through. The electrolyte serves to conduct lithium ions between the positive electrode sheet and the negative electrode sheet. The secondary battery of the present application may be a lithium-containing secondary battery, and in particular, may be a lithium-ion secondary battery. [Negative electrode]

[0136] The negative electrode plate used in the secondary battery of the present application is the negative electrode plate of any embodiment of the third aspect of the present application. [Positive electrode]

[0137] In some embodiments, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector. For example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0138] The positive electrode film layer includes a positive electrode active material, and the positive electrode active material can adopt a positive electrode active material for a secondary battery known in the art. For example, the positive electrode active material may include a combination of one or more selected from lithium transition metal oxides, lithium phosphates containing olivine structures, and their respective modified compounds. Examples of lithium transition metal oxides may include a combination of one or more selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium phosphates containing olivine structures may include a combination of one or more selected from lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.

[0139] In some embodiments, in order to further improve the energy density of the secondary battery, the positive electrode active material may include a combination of one or more of the lithium transition metal oxides shown in Formula 1 and modified compounds thereof.

[0140] Li a Ni b Co c M d O e A f Formula 1

[0141] In Formula 1, 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes a combination of one or more selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes a combination of one or more selected from N, F, S and Cl.

[0142] In the present application, the modified compound of each positive electrode active material mentioned above may be a compound obtained by doping and / or surface coating the positive electrode active material.

[0143] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application has no particular restrictions on the type of the positive electrode conductive agent. As an example, the positive electrode conductive agent includes a combination of one or more selected from superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the positive electrode conductive agent is less than 5%.

[0144] In some embodiments, the positive electrode film layer may also optionally include a positive electrode binder. The present application has no particular restrictions on the type of the positive electrode binder. As an example, the positive electrode binder may include a combination of one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin. In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the positive electrode binder is less than 5%.

[0145] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, an aluminum foil or an aluminum alloy foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include a combination of one or more selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, and the polymer material base layer may include a combination of one or more selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).

[0146] The positive electrode film layer is usually formed by coating the positive electrode slurry on the positive electrode current collector, drying and cold pressing. The positive electrode slurry is usually formed by dispersing the positive electrode active material, optional conductive agent, optional binder and any other components in a solvent and stirring them uniformly. The solvent can be N-methylpyrrolidone (NMP), but is not limited thereto. [Electrolyte]

[0147] The electrolyte of the present application can be an electrolyte for secondary batteries known in the art. The electrolyte includes a lithium salt and an organic solvent.

[0148] As an example, the lithium salt may include a combination of one or more selected from lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0149] As an example, the organic solvent may include a combination of one or more selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE). [Isolation film]

[0150] The present application has no particular limitation on the type of the isolation membrane, and any known porous structure isolation membrane with good chemical stability and mechanical stability can be selected.

[0151] In some embodiments, the material of the isolation membrane may include a combination of one or more selected from glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer are the same or different.

[0152] In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly by a winding process or a lamination process.

[0153] In some embodiments, the secondary battery may include an outer package, which may be used to package the electrode assembly and the electrolyte.

[0154] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as a combination of one or more of polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS).

[0155] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 2 The secondary battery 5 is a square structure as an example.

[0156] In some embodiments, Figure 3 As shown, the outer package may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are enclosed to form a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation film can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.

[0157] The preparation method of the secondary battery of the present application is well known. In some embodiments, the positive electrode sheet, the separator, the negative electrode sheet and the electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, the separator and the negative electrode sheet can be formed into an electrode assembly through a winding process or a lamination process, and the electrode assembly is placed in an outer package, and the electrolyte is injected after drying, and the secondary battery is obtained through vacuum packaging, standing, forming, shaping and other processes.

[0158] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.

[0159] Figure 4 FIG. 4 is a schematic diagram of a battery module 4 as an example. Figure 4 As shown, in the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0160] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0161] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.

[0162] Figure 5 and Figure 6 FIG. 1 is a schematic diagram of a battery pack 1 as an example. Figure 5 and Figure 6 As shown, the battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3, wherein the upper box body 2 is used to cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner. Electrical devices

[0163] The fifth aspect of the embodiment of the present application provides an electric device, which includes at least one of the secondary battery, battery module and battery pack of the present application. The secondary battery, battery module and battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.

[0164] The electrical device may select a secondary battery, a battery module or a battery pack according to its usage requirements.

[0165] Figure 7Schematic diagram of an electric device as an example. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the requirements of the electric device for high power and high energy density, a battery pack or a battery module may be used.

[0166] As another example, the electric device may be a mobile phone, a tablet computer, a notebook computer, etc. The electric device is usually required to be light and thin, and a secondary battery may be used as a power source. Example

[0167] The following examples describe the disclosure of the present application in more detail, and these examples are only for illustrative purposes, as it is obvious to those skilled in the art that various modifications and variations can be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages and ratios reported in the following examples are based on mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further treatment, and the instruments used in the examples are commercially available. Example 1

[0168] Step (1): Preparation of negative electrode active material

[0169] S10, delaying coking petroleum residue at 490℃~510℃ to obtain petroleum non-needle coke green coke; crushing, shaping and grading the green coke to obtain coke powder; mixing the obtained coke powder with coal tar as a binder, and then granulating; placing the obtained granulated product in a graphite crucible, and then placing the graphite crucible in an Acheson graphitization furnace, filling resistor material around the graphite crucible, turning on electricity to make current flow through the resistor material to generate heat energy, and performing graphitization treatment at about 3000℃ for about 30h to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8μm, and the degree of graphitization is about 92%.

[0170] S20, the obtained artificial graphite particles are uniformly mixed with carbon source petroleum asphalt (the added mass is calculated as residual carbon value) and ferroelectric material BaTiO3 (volume average particle size Dv50 is 200nm, dielectric constant is 2000) according to a mass ratio of 100:3:3, and then carbonized and sintered in a track kiln, the temperature in the highest temperature zone is about 1150°C, and the operation time in the highest temperature zone is about 12h, so as to form an amorphous carbon coating layer on at least a part of the surface of the artificial graphite particles to obtain a negative electrode active material. In the obtained negative electrode active material, BaTiO3 is dispersed in the coating layer and at least part of the BaTiO3 protrudes from the surface of the coating layer.

[0171] Step (2): Preparation of negative electrode sheet

[0172] The negative electrode active material prepared above, binder styrene butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black were fully stirred and mixed in a proper amount of solvent deionized water at a mass ratio of 96.8:1.2:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry was evenly coated on the surface of the negative electrode current collector copper foil, and after drying and cold pressing, a negative electrode sheet was obtained. The coating amount was 0.162kg / m 2 , compacted density is 1.65g / cm 3 .

[0173] Step (3): Preparation of positive electrode

[0174] The positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in a proper amount of solvent NMP at a mass ratio of 96.2:1.8:2 to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained. The coating amount is 0.256kg / m 2 , compacted density is 3.4g / cm 3 .

[0175] Step (4): Preparation of electrolyte

[0176] Ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.

[0177] Step (5): Preparation of isolation membrane

[0178] A porous polyethylene membrane was used as the separator.

[0179] Step (6): Preparation of secondary battery

[0180] The positive electrode sheet, the separator, and the negative electrode sheet are stacked and wound in order to obtain an electrode assembly; the electrode assembly is placed in an outer package, and after drying, the electrolyte is injected, and after vacuum packaging, standing, forming, shaping and other processes, a secondary battery is obtained. Examples 2 to 16

[0181] The secondary batteries of Examples 2 to 16 were prepared in a similar manner to that of Example 1, except that the relevant parameters in “Preparation of negative electrode active material” were adjusted. The specific parameters are shown in Table 2. Comparative Example 1

[0182] The secondary battery of Comparative Example 1 was prepared in a similar manner to that of Example 1, except that conventional artificial graphite without a coating layer was used as the negative electrode active material. Specifically, the artificial graphite was prepared in the following manner.

[0183] The petroleum residue is subjected to delayed coking at 490℃~510℃ to obtain petroleum non-needle coke green coke; the green coke is crushed, shaped and graded to obtain coke powder; the obtained coke powder is mixed with the binder coal tar, and then granulated; the obtained granulated product is placed in a graphite crucible, and then the graphite crucible is placed in an Acheson graphitization furnace, and resistor materials are filled around the graphite crucible, and current is passed through the resistor materials to generate heat energy, and graphitization treatment is performed at about 3000℃ for about 30 hours to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8μm, and the degree of graphitization is about 92%. Comparative Example 2

[0184] The secondary battery of Comparative Example 2 was prepared in a similar manner to that of Example 1, except that the negative electrode active material was prepared in the following manner.

[0185] S10, delaying coking petroleum residue at 490℃~510℃ to obtain petroleum non-needle coke green coke; crushing, shaping and grading the green coke to obtain coke powder; mixing the obtained coke powder with coal tar as a binder, and then granulating; placing the obtained granulated product in a graphite crucible, and then placing the graphite crucible in an Acheson graphitization furnace, filling resistor material around the graphite crucible, turning on electricity to make current flow through the resistor material to generate heat energy, and performing graphitization treatment at about 3000℃ for about 30h to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8μm, and the degree of graphitization is about 92%.

[0186] S20, mixing the obtained artificial graphite particles with the carbon source petroleum asphalt and then performing carbonization sintering treatment in a track kiln, wherein the temperature in the highest temperature zone is about 1150° C. and the operation time in the highest temperature zone is about 12 hours, so as to form an amorphous carbon coating layer on at least a portion of the surface of the artificial graphite particles to obtain a negative electrode active material. Comparative Example 3

[0187] The secondary battery of Comparative Example 3 was prepared in a similar manner to that of Example 1, except that the negative electrode active material and the negative electrode sheet were prepared in the following manner.

[0188] Step (1): Preparation of negative electrode active material

[0189] S10, delaying coking petroleum residue at 490℃~510℃ to obtain petroleum non-needle coke green coke; crushing, shaping and grading the green coke to obtain coke powder; mixing the obtained coke powder with coal tar as a binder, and then granulating; placing the obtained granulated product in a graphite crucible, and then placing the graphite crucible in an Acheson graphitization furnace, filling resistor material around the graphite crucible, turning on electricity to make current flow through the resistor material to generate heat energy, and performing graphitization treatment at about 3000℃ for about 30h to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8μm, and the degree of graphitization is about 92%.

[0190] S20, mixing the obtained artificial graphite particles with the carbon source petroleum asphalt and then performing carbonization sintering treatment in a track kiln, wherein the temperature in the highest temperature zone is about 1150° C. and the operation time in the highest temperature zone is about 12 hours, so as to form an amorphous carbon coating layer on at least a portion of the surface of the artificial graphite particles to obtain a negative electrode active material.

[0191] Step (2): Preparation of negative electrode sheet

[0192] The negative electrode active material prepared above, ferroelectric material BaTiO3 (volume average particle size Dv50 is 85nm), binder styrene-butadiene rubber (SBR), thickener sodium carboxymethyl cellulose (CMC-Na), and conductive agent carbon black are fully stirred and mixed in a proper amount of solvent deionized water in a mass ratio of 93.8:3:1.2:1.2:0.8 to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on the surface of the negative electrode collector copper foil, and after drying and cold pressing, a negative electrode sheet is obtained. Comparative Example 4

[0193] The secondary battery of Comparative Example 4 was prepared in a similar manner to that of Example 1, except that the negative electrode active material was prepared in the following manner.

[0194] S10, delaying coking petroleum residue at 490℃~510℃ to obtain petroleum non-needle coke green coke; crushing, shaping and grading the green coke to obtain coke powder; mixing the obtained coke powder with coal tar as a binder, and then granulating; placing the obtained granulated product in a graphite crucible, and then placing the graphite crucible in an Acheson graphitization furnace, filling resistor material around the graphite crucible, turning on electricity to make current flow through the resistor material to generate heat energy, and performing graphitization treatment at about 3000℃ for about 30h to obtain artificial graphite particles. The volume average particle size Dv50 of the artificial graphite particles is about 9.8μm, and the degree of graphitization is about 92%.

[0195] S20, mixing the obtained artificial graphite particles with the carbon source petroleum asphalt and then performing carbonization sintering treatment in a track kiln, wherein the temperature in the highest temperature zone is about 1150° C. and the operation time in the highest temperature zone is about 12 hours, so as to form an amorphous carbon coating layer on at least a portion of the surface of the artificial graphite particles.

[0196] S30, the obtained artificial graphite particles with an amorphous carbon coating layer and the ferroelectric material BaTiO3 (volume average particle size Dv50 is 85nm) are evenly mixed by ball milling in a mass ratio of 97:3, and then put into a planetary ball mill. After ball milling for 2h at an ambient temperature of 25°C and a rotation speed of 300 rpm, the negative electrode active material is obtained. Test Section

[0197] (1) Volume average particle size Dv50 test

[0198] A certain amount of the negative electrode active material sample prepared above was taken and the volume average particle size Dv50 was tested by a Mastersizer 2000E laser particle size analyzer. The test standard was based on GB / T 19077-2016.

[0199] (2) Specific surface area test

[0200] A certain amount of the negative electrode active material sample prepared above was taken and the specific surface area was tested by a Tri-Star 3020 specific surface area pore size analyzer from Micromeritics, USA. The specific surface area was calculated by the BET (Brunauer Emmett Teller) method. The test standard was based on GB / T 19587-2017.

[0201] (3) Powder compaction density test

[0202] Take a certain amount of the negative electrode active material sample prepared above and add it to the bottom area of ​​1.327cm of UTM7305 electronic pressure testing machine. 2 The mold is pressurized to 2000kg (equivalent to 20000N), maintained for 30s, then released, maintained for 10s, and then the powder compaction density of the negative electrode active material under a force of 20000N is recorded and calculated. The test standard is based on GB / T24533-2009.

[0203] (4) Graphitization degree test

[0204] A certain amount of the negative electrode active material sample prepared above was taken and tested using a Bruker D8 Discover X-ray diffractometer to obtain the interlayer spacing d of the (002) crystal plane of the coating layer and the carbon-based material particles, respectively. 002 Then according to the formula g = (0.344-d 002) / (0.344-0.3354)×100%, and the graphitization degree g1 of the coating layer and the graphitization degree g2 of the carbon-based material particles are calculated. The test standard is based on JIS K 0131-1996 and JB / T 4220-2011.

[0205] (5) Average thickness test of coating layer

[0206] Take a certain amount of the negative electrode active material sample prepared as above, cut a thin slice of about 100 nm from the middle of a single particle, and then perform transmission electron microscopy analysis on the thin slice to obtain a TEM image. Then measure the thickness at multiple (for example, more than 5) different positions on the TEM image, and test at least 6 negative electrode active material samples, and take the average value of the test results as the average thickness of the coating layer.

[0207] (6) Initial gram capacity test

[0208] The negative electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) prepared above are mixed evenly in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 91.6:1.8:6.6 to prepare a slurry; the prepared slurry is coated on a copper foil, dried in an oven and set aside; then a metal lithium sheet is used as a counter electrode, a polyethylene (PE) film is used as an isolation membrane, a few drops of the same electrolyte as the above secondary battery are dripped, and a CR2430 button battery is assembled in an argon-protected glove box.

[0209] After the button cell was left to stand for 12 hours, it was discharged at 0.05C constant current to 0.005V at 25°C, left to stand for 10 minutes, and then discharged at 50μA constant current to 0.005V, left to stand for 10 minutes, and then discharged at 10μA constant current to 0.005V; then it was charged at 0.1C constant current to 2V, and the charging capacity was recorded. The ratio of the charging capacity to the mass of the negative electrode active material is the initial gram capacity of the negative electrode active material.

[0210] (7) Secondary battery fast charging performance test

[0211] At 25°C, the prepared secondary battery was charged at a constant current of 0.33C to a charge cut-off voltage of 4.4V, then charged at a constant voltage to a current of 0.05C, allowed to stand for 5 minutes, and then discharged at a constant current of 0.33C to a discharge cut-off voltage of 2.8V, and its actual capacity was recorded as C0.

[0212] Then the secondary battery is charged with constant current of 0.5C0, 1C0, 1.5C0, 2C0, 2.5C0, 3C0, 3.5C0, 4C0, 4.5C0 in sequence to the full battery charge cut-off voltage of 4.4V or 0V negative electrode cut-off potential (whichever is reached first). After each charge is completed, it is necessary to discharge with 1C0 to the full battery discharge cut-off voltage of 2.8V. Record the state of charge (SOC) at different charge rates to 10%, 20%, 30% ... 80% The negative electrode potential corresponding to the state of charge (SOC) is plotted, and the rate-negative electrode potential curve under different SOC states is obtained after linear fitting. The charge rate corresponding to the negative electrode potential of 0V under different SOC states is obtained. The charge rate is the charging window under the SOC state, which is recorded as C10% SOC, C20% SOC, C30% SOC, C40% SOC, C50% SOC, C60% SOC, C70% SOC, and C80% SOC respectively. The charging time T of the secondary battery from 10% SOC to 80% SOC is calculated according to the formula (60 / C20% SOC+60 / C30% SOC+60 / C40% SOC+60 / C50% SOC+60 / C60% SOC+60 / C70% SOC+60 / C80% SOC)×10%. The shorter the charging time T, the better the fast charging performance of the secondary battery.

[0213] (8) Cyclic performance test

[0214] At 25°C, the secondary battery prepared above was charged at a constant current of 0.33C to a charge cut-off voltage of 4.4V, then charged at a constant voltage to a current of 0.05C, left to stand for 5 minutes, and then discharged at a constant current of 0.33C to a discharge cut-off voltage of 2.8V, and its initial capacity was recorded as C0. Then, the battery was charged according to the strategy shown in Table 1, discharged at 0.33C, and the discharge capacity Cn of each cycle was recorded until the cycle capacity retention rate (i.e., Cn / C0×100%) was 80%, and the number of cycles was recorded. The more cycles, the better the cycle performance of the secondary battery. Table 1 State of charge SOC of secondary battery Charging rate (C) 0~10% 0.33 10%~20% 5.2 20%~30% 4.5 30%~40% 4.2 40%~50% 3.3 50%~60% 2.6 60%~70% 2.0 70%~80% 1.5 80%~100% 0.33

[0215] Table 2 shows the preparation parameters of the negative electrode active materials of Examples 1 to 16.

[0216] Table 3 shows the test results of Examples 1 to 16 and Comparative Examples 1 to 4 obtained according to the above performance testing method.

[0217] From the test results in Table 3, it can be seen that the negative electrode active material of the present application has good kinetic properties, can shorten the fast charging time of the secondary battery, and extend the cycle life of the secondary battery without sacrificing the high gram capacity of the negative electrode active material.

[0218] Compared with Comparative Example 1, Comparative Example 2 uses amorphous carbon-coated artificial graphite as the negative electrode active material, which can improve the fast charging performance and cycle performance of the secondary battery to a certain extent, but the improvement effect is limited and cannot meet people's requirements for higher fast charging capability and longer cycle life of secondary batteries.

[0219] Compared with Comparative Example 2, Comparative Example 3 further adds ferroelectric materials to the negative electrode slurry, thereby further improving the fast charging performance and cycle performance of the secondary battery, but the improvement effect is limited and cannot meet people's requirements for higher fast charging capacity and longer cycle life of the secondary battery. The possible reason is that by physically mixing the ferroelectric material in the negative electrode slurry, on the one hand, due to the high density of the ferroelectric material, it is easy to settle in the negative electrode slurry, and it is difficult to form a stable negative electrode slurry, which affects the production rate and the quality of the negative electrode sheet; on the other hand, the addition of ferroelectric materials by physical mixing will cause part of the ferroelectric material and the negative electrode active material to not form physical contact in the negative electrode sheet, and thus the role of the ferroelectric material cannot be played, resulting in limited improvement of the fast charging performance and cycle performance of the secondary battery.

[0220] Compared with Comparative Example 1, Comparative Example 4 uses artificial graphite coated with barium titanate as the negative electrode active material, but the negative electrode active material is obtained by direct ball milling, which improves the fast charging performance and cycle performance of the secondary battery to a certain extent compared with Comparative Example 1, but the improvement effect is limited and cannot meet people's requirements for higher fast charging capacity and longer cycle life of the secondary battery. The possible reason is that, on the one hand, the direct ball milling method is to form a negative electrode active material by colliding and grinding the artificial graphite particles and the ferroelectric material particles, but the high-energy ball milling will destroy the morphology of the formed artificial graphite particles, which may cause the surface amorphous carbon coating layer to fall off, affecting the fast charging performance of the negative electrode active material. On the other hand, after the surface of the negative electrode active material is destroyed, the electrolyte (especially the solvent) will be embedded in the negative electrode active material, increasing the irreversible consumption of active lithium ions, thereby reducing the cycle performance of the secondary battery.

[0221] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A fast-charge type negative electrode active material, wherein: The fast-charging anodic active material includes carbon-based material particles, a coating layer located on at least a part of the surface of the carbon-based material particles, and a ferroelectric material dispersed in the coating layer. The coating layer includes a conductive carbon material, and at least a part of the ferroelectric material protrudes from the surface of the coating layer. Wherein, the mass ratio of the ferroelectric material to the carbon-based material particles is α1, α1 is (0.5 to 10):100, and / or, the mass ratio of the coating layer to the carbon-based material particles is α2, α2 is (2 to 10):

100.

2. The fast-charging negative electrode active material according to claim 1, wherein: The average thickness of the coating layer is H nm, the volume average particle size Dv50 of the ferroelectric material is d1 nm, and the fast-charging anodic active material satisfies: 0.25 ≤ H / d1 ≤ 1.

1. Optionally, 0.25 ≤ H / d1 ≤ 0.

5.

3. The fast-charging negative electrode active material according to any one of claims 1 to 2, wherein: The volume average particle size Dv50 of the ferroelectric material is d1 nm, 0 < d1 ≤ 200. Optionally, 0 < d1 ≤ 100; and / or, The average thickness of the coating layer is H nm, 20 ≤ H ≤ 100. Optionally, 20 ≤ H ≤ 50.

4. The fast-charging negative electrode active material according to any one of claims 1 to 3, wherein α1 is (1-3):100; and / or α2 is (2-5):

100.

5. The fast-charging negative electrode active material according to any one of claims 1 to 4, wherein: The mass ratio of the ferroelectric material to the carbon-based material particles is α1, the mass ratio of the coating layer to the carbon-based material particles is α2, and α1:α2 is 1:6 to 4:

1. Optionally, it is 1:4 to 2:

1.

6. The fast-charging negative electrode active material according to any one of claims 1 to 5, wherein: The graphitization degree of the coating layer is 45% to 80%; and / or, The graphitization degree of the carbon-based material particles is 88% to 96%.

7. The fast-charging negative electrode active material according to any one of claims 1 to 6, wherein: The volume average particle size Dv50 of the carbon-based material particles is d2 μm, 5 ≤ d2 ≤ 20. Optionally, 8 ≤ d2 ≤ 15.

8. The fast-charging negative electrode active material according to any one of claims 1 to 7, wherein: The morphology of the carbon-based material particles is primary particles, secondary particles or a combination thereof. Optionally, in the carbon-based material particles with the morphology of secondary particles, the ratio of the volume average particle size Dv50 of the primary particles to the volume average particle size Dv50 of the secondary particles formed by them is 0.2 to 0.

5.

9. The fast-charging negative electrode active material according to any one of claims 1 to 8, wherein: The dielectric constant of the ferroelectric material is above 100. Optionally, it is 100 to 100000; and / or, The Curie temperature of the ferroelectric material is above 80°C.

10. The fast-charging negative electrode active material according to any one of claims 1 to 9, wherein: The carbon-based material particles include one or more combinations selected from graphite, mesocarbon microbeads, hard carbon, and soft carbon. Optionally, it is selected from graphite; and / or, The conductive carbon material in the coating layer includes amorphous carbon. Optionally, it includes hard carbon; and / or, The ferroelectric material includes one or more combinations selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate, and lithium tantalate.

11. The fast-charging negative electrode active material according to any one of claims 1 to 10, wherein: The fast-charging anodic active material satisfies at least one of the following conditions (1) to (3): (1) The volume average particle size Dv50 of the fast-charging anodic active material is 5 μm to 20 μm. Optionally, it is 8 μm to 15 μm. (2) The specific surface area of ​​the fast-charging negative electrode active material is 0.8 m 2 / g to 1.3m 2 / g, optionally 0.9m 2 / g to 1.2m 2 / g; (3) The powder compaction density of the fast-charging negative electrode active material under a force of 20,000 N is 1.5 g / cm 3 Up to 1.9g / cm 3 , optionally 1.5 g / cm 3 Up to 1.7g / cm 3 .

12. A method for preparing a fast-charging negative electrode active material, comprising the steps of: S10, providing carbon-based material particles, a carbon source and a ferroelectric material, optionally, the carbon source comprises a combination of one or more selected from asphalt, resin, and biomass materials; S20, uniformly mixing the carbon-based material particles, the carbon source and the ferroelectric material, and forming a coating layer including a conductive carbon material on at least a portion of the surface of the carbon-based material particles through carbonization and sintering, wherein: The ferroelectric material is dispersed in the coating layer and at least a part of the ferroelectric material protrudes from the surface of the coating layer.

13. The method according to claim 12, wherein: The carbonization sintering temperature in S20 is 700°C to 1800°C. Optionally, it is 1000°C to 1300°C; and / or, The carbonization sintering time in S20 is 1 h to 15 h. Optionally, it is 6 h to 14 h.

14. The method according to any one of claims 12 to 13, wherein: The carbon-based material particles are prepared by the following method: S101, providing coke powder, and placing the coke powder into a reaction container; S102, graphitizing the coke powder to obtain carbon-based material particles.

15. A negative electrode sheet, comprising a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein: The negative electrode film layer comprises the fast-charging negative electrode active material according to any one of claims 1 to 11 or the fast-charging negative electrode active material prepared by the method according to any one of claims 12 to 14. 16 . A secondary battery comprising the negative electrode sheet according to claim 15 .

17. An electrical device comprising the secondary battery according to claim 16.

Citation Information

Patent Citations

  • Method for testing dielectric constant of barium titanate powder

    CN114217139A

  • In-situ composite lithium battery negative electrode material and preparation method and application thereof

    CN110034280A

  • Carbon electrode for polymer battery and the polymer battery using the same

    JP2004193041A

  • Composite carbon particles, method for producing same, and lithium ion secondary battery

    WO2020105599A1