Prepreg, laminated board, printed wiring board, and semiconductor package
By forming a thermosetting resin region with low energy storage modulus and high energy storage modulus in the prepreg, combined with a fiber substrate, the warping change and conductor adhesion balance caused by the difference in thermal expansion rate of the insulating material of printed circuit board are solved. The problem has improved the connection reliability of semiconductor packages.
Patent Information
- Application Number
- CN202280095478.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-06
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to find a balance between improving the amount of warping change caused by the difference in thermal expansion rate of insulating materials of printed circuit boards and conductor adhesion, resulting in a reduction in connection reliability of semiconductor packages.
Using prepregs with different thermosetting resin composition areas, the warpage variation is reduced and maintained by forming a first area of low energy storage modulus and a second area of high energy storage modulus on the surface. Conductor adhesion.
The warping change of semiconductor package is effectively reduced, while maintaining a prepreg with good conductor adhesion. It is used in laminated boards, printed circuit boards and semiconductor packages, improving the connection reliability of the package.
Smart Images

Figure CN119095902A_ABST
Abstract
Description
Technical Field
[0001] The present embodiment relates to a prepreg, a laminate, a printed wiring board, and a semiconductor package. Background Art
[0002] In recent years, along with the trend of miniaturization and higher performance of electronic devices, printed wiring boards are being advanced in terms of higher wiring density and higher integration.
[0003] As the insulating material of the printed circuit board, the thermosetting resin is mainly used. Although the thermosetting resin has excellent insulation and heat resistance, it has a larger thermal expansion coefficient than inorganic components such as semiconductor elements and circuits, so there is a situation where the warping caused by the difference in thermal expansion coefficient with the inorganic components becomes a problem.
[0004] When a semiconductor chip is mounted on the surface of a printed wiring board, the difference between the warpage of the semiconductor package at room temperature and the warpage at the reflow soldering temperature (hereinafter also referred to as "warpage variation") becomes larger due to the difference in thermal expansion coefficient. This increase in warpage variation becomes a factor that reduces the connection reliability of the semiconductor package.
[0005] As a method for reducing the thermal expansion coefficient of the insulating material, for example, a method of filling a thermosetting resin with an inorganic filler at a high density has been proposed (for example, see Patent Document 1). By filling with an inorganic filler having a low thermal expansion coefficient at a high density, the difference in thermal expansion coefficient between the insulating material containing the thermosetting resin and an inorganic component such as a semiconductor element can be reduced.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2020-059820 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, high filling of inorganic fillers may cause the adhesion between the insulating material and the conductor layer (hereinafter also referred to as "conductor adhesion") to decrease. Therefore, from the perspective of ensuring a good balance with the conductor adhesion, the method for improving the warpage based on high filling of inorganic fillers has a limit.
[0011] In view of such a situation, the present embodiment aims to provide a prepreg which can reduce the warpage variation of a semiconductor package and has excellent conductor adhesion, and a laminate, a printed wiring board and a semiconductor package using the prepreg.
[0012] Means for solving problems
[0013] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by the present embodiment described below.
[0014] That is, this embodiment relates to the following [1] to
[12] .
[0015] [1] A prepreg comprising a thermosetting resin composition and a fiber base material,
[0016] The prepreg has one surface and another surface on the opposite side to the one surface.
[0017] The prepreg has, starting from at least one of the one surface and the other surface and in a surface direction opposite to the surface serving as the starting point, the following components in order:
[0018] a first region constituting the surface of the prepreg serving as the starting point and containing a thermosetting resin composition; and
[0019] The second region is a region containing a thermosetting resin composition different from the thermosetting resin composition contained in the first region.
[0020] The storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region is lower than the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region.
[0021] [2] The prepreg according to the above [1], wherein the above prepreg has the above first region and the above second region in sequence in the surface direction toward the opposite side of the surface serving as the starting point, with each surface of the above one surface and the above another surface as the starting point.
[0022] [3] A prepreg according to [1] or [2] above, wherein the difference between the storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region and the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region [E'(2)-E'(1)] is 0.05 to 1.5 GPa.
[0023] [4] The prepreg according to any one of [1] to [3] above, wherein the storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region is 0.1 to 1.5 GPa.
[0024] [5] The prepreg according to any one of [1] to [4] above, wherein the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region is 0.5 to 2.0 GPa.
[0025] [6] The prepreg according to any one of [1] to [5], wherein the thermosetting resin composition contained in the first region and the thermosetting resin composition contained in the second region contain an inorganic filler.
[0026] The volume-based content V(1) of the inorganic filler in the thermosetting resin composition in the first region is lower than the volume-based content V(2) of the inorganic filler in the thermosetting resin composition in the second region.
[0027] [7] The prepreg according to [6] above, wherein the difference [V(2)-V(1)] between the volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region and the volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region is 2 to 40% by volume.
[0028] [8] The prepreg according to any one of [1] to [7] above, wherein the volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region is 5 to 60% by volume.
[0029] [9] The prepreg according to any one of [1] to [8] above, wherein the volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region is 20 to 80% by volume.
[0030]
[10] A laminate comprising a cured product of the prepreg according to any one of [1] to [9] above and a metal foil.
[0031]
[11] A printed wiring board comprising a cured product of the prepreg according to any one of [1] to [9] above.
[0032]
[12] A semiconductor package comprising the printed wiring board described in
[11] above and a semiconductor element.
[0033] Effects of the Invention
[0034] According to the present embodiment, it is possible to provide a prepreg that can reduce the amount of warpage change of a semiconductor package and has excellent conductor adhesion, and a laminated board, a printed wiring board, and a semiconductor package using the prepreg. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a schematic cross-sectional view showing an example of the prepreg according to the present embodiment.
[0036] Figure 2 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0037] Figure 3 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0038] Figure 4 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0039] Figure 5 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0040] Figure 6 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0041] Figure 7 This is a schematic cross-sectional view showing another example of the prepreg according to the present embodiment.
[0042] Figure 8 This is a schematic cross-sectional view for explaining the structure of the prepreg of the example. DETAILED DESCRIPTION
[0043] In the present specification, a numerical range expressed using "to" indicates a range including the numerical values described before and after "to" as the minimum value and the maximum value, respectively.
[0044] For example, a numerical range such as "X to Y" (X and Y are real numbers) means a numerical range of more than X and less than Y. Furthermore, a description such as "more than X" in this specification means X and a numerical value greater than X. In addition, a description such as "less than Y" in this specification means Y and a numerical value less than Y.
[0045] The lower limit value and the upper limit value of the numerical range described in the present specification can be arbitrarily combined with the lower limit value or the upper limit value of other numerical ranges, respectively.
[0046] In the numerical range described in the present specification, the lower limit value or the upper limit value of the numerical range may be replaced with the value shown in the Examples.
[0047] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0048] In the present specification, when a plurality of substances corresponding to each component are present in the resin composition, the content of each component in the resin composition means the total amount of the plurality of substances present in the resin composition unless otherwise specified.
[0049] The term "solid content" as used herein refers to components other than the solvent, and also includes components that are liquid, syrupy, or waxy at room temperature. Here, room temperature as used herein means 25°C.
[0050] The "semi-cured product" in this specification is synonymous with the resin composition in the B-stage state in JIS K 6800 (1985), and the "cured product" is synonymous with the resin composition in the C-stage state in JIS K 6800 (1985).
[0051] The action mechanism described in this specification is a guess, and does not limit the mechanism by which the effects of the present embodiment are achieved.
[0052] The present embodiment also includes any combination of the matters described in this specification.
[0053] [Prepreg]
[0054] The prepreg of the present embodiment is a prepreg comprising a thermosetting resin composition and a fiber base material.
[0055] The prepreg has one surface and another surface on the opposite side to the one surface.
[0056] The prepreg has, starting from at least one of the one surface and the other surface and in a surface direction opposite to the surface serving as the starting point, the following components in order:
[0057] a first region constituting the surface of the prepreg serving as the starting point and containing a thermosetting resin composition; and
[0058] The second region is a region containing a thermosetting resin composition different from the thermosetting resin composition contained in the first region.
[0059] The storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region is lower than the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region.
[0060] The reason why the prepreg of the present embodiment can reduce the amount of warpage change of the semiconductor package and has excellent conductor adhesion is not certain, but can be inferred as follows.
[0061] The prepreg of this embodiment has, starting from at least one surface and in the surface direction toward the opposite side of the surface serving as the starting point, a first region containing a thermosetting resin composition having a relatively low storage modulus E' of the cured product at 260°C (hereinafter also referred to as "260°C storage modulus E'"); and a second region containing a thermosetting resin composition having a relatively high storage modulus E' of the cured product at 260°C.
[0062] It can be considered that the cured product of the thermosetting resin composition contained in the first region has a low storage modulus E' at 260°C, thus relieving the stress caused by the difference in thermal expansion coefficient between the cured product and the inorganic components such as the semiconductor chip mounted on the first region. In addition, it can be inferred that since the storage modulus E' at 260°C of the thermosetting resin composition contained in the second region is high, the cured product in the second region increases the rigidity of the cured product of the prepreg, thereby reducing the warpage change of the semiconductor package. That is, it can be considered that the prepreg of this embodiment can reduce the warpage change by stress relief and rigidity even if the inorganic filler is not highly filled as described above, so the conductor adhesion can be well maintained.
[0063] The prepreg of this embodiment only needs to have the above-mentioned first region and the above-mentioned second region in sequence in the surface direction opposite to the surface serving as the starting point, starting from at least any one of the above-mentioned one surface and the above-mentioned other surface. However, it is preferred that the above-mentioned first region and the above-mentioned second region be respectively started from the above-mentioned one surface and the above-mentioned other surface, and be sequentially provided in the surface direction opposite to the surface serving as the starting point.
[0064] Hereinafter, the form of the prepreg according to the present embodiment will be described in detail with reference to the drawings.
[0065] <Prepreg Form>
[0066] Examples of the form of the prepreg of this embodiment include: Figures 1 to 3 The morphology of the prepregs 10, 20 and 30 shown. It should be noted that Figures 1 to 3 In the figure, the fiber base material is omitted.
[0067] Figure 1 The prepreg 10 of the first embodiment shown has a first region 1 and a second region 2 in this order, starting from one surface Sα and extending in a direction x toward the other surface Sβ.
[0068] The first region 1 constitutes one surface Sα of the prepreg 10 , and the second region 2 constitutes the other surface Sβ of the prepreg 10 .
[0069] The first region and the second region of the prepreg of the present embodiment are preferably as follows, for example Figure 1The layers are formed like the prepreg 10 shown. It should be noted that there may not be a clear interface between adjacent layers, and for example, part of the constituent components of the first region may be compatible or mixed with part of the constituent components of the second region.
[0070] Figure 2 The prepreg 20 of the second embodiment shown has a first region 1 and a second region 2 in sequence from one surface Sα as a starting point and in a direction X1 toward another surface Sβ, and has another first region 1 and a second region 2 in sequence from another surface Sβ as a starting point and in a direction X2 toward one surface Sα. In other words, the prepreg 20 has a first region 1, a second region 2, and a first region 1 in sequence.
[0071] In the prepreg 20 , the first region 1 constitutes one surface Sα and the other surface Sβ of the prepreg 20 .
[0072] Figure 3 The prepreg 30 of the third embodiment shown has a first region 1, a second region 2, and a third region 3 in sequence from one surface Sα as a starting point and in a direction X1 toward another surface Sβ, and has another first region 1 and another second region 2 and a third region 3 in sequence from another surface Sβ as a starting point and in a direction X2 toward one surface Sα. In other words, the prepreg 30 has a first region 1, a second region 2, a third region 3, a second region 2, and a first region 1 in sequence.
[0073] In the prepreg 30 , the first region 1 constitutes one surface Sα and the other surface Sβ of the prepreg 30 .
[0074] The third region 3 is a region containing a third thermosetting resin composition, and the storage modulus E' of the cured product of the third thermosetting resin composition at 260°C is lower than the storage modulus E'(2) of the cured product of the thermosetting resin composition contained in the second region 2 at 260°C.
[0075] The prepreg of this embodiment is preferably Figure 2 The prepreg 20 shown, Figure 3 Like the prepreg 30 shown in the figure, the first region and the second region are sequentially provided with one surface and the other surface as starting points respectively, and in the surface direction opposite to the surface serving as the starting point.
[0076] In the present embodiment, the prepreg is, for example, Figure 2 The prepreg 20 and Figure 3 When there are two or more first regions like the prepreg 30 shown, the composition, thickness, etc. of the two or more first regions may be the same or different.
[0077] In the present embodiment, the prepreg is, for example, Figure 3 When there are two or more second regions like the prepreg 30 shown, the composition, thickness, etc. of the two or more second regions may be the same or different.
[0078] It should be noted that in the following description, various suitable forms of the first region regarding the storage modulus, thickness, composition, etc., when the prepreg of this embodiment has more than two first regions, preferably all of the first regions are of the suitable form, but only a part of the first regions among more than two first regions may be of the suitable form.
[0079] Similarly, in the following description, various suitable forms of the second region such as storage modulus, thickness, composition, etc., when the prepreg of the present embodiment has two or more second regions, preferably all of the second regions are the suitable forms, but only a part of the second regions among the two or more second regions may be the suitable forms. The same is true when the prepreg of the present embodiment has two or more third regions.
[0080] <Position of Fiber Base Material in Prepreg>
[0081] In the prepreg of the present embodiment, the position of the fiber base material is not particularly limited, but the fiber base material is preferably included in the second region.
[0082] That is, the second region is preferably a region containing a thermosetting resin composition and a fiber base material. In this case, the fiber base material may be partially contained in the second region or entirely contained in the second region.
[0083] Figure 4 and Figure 5 2 is a schematic cross-sectional view of a fiber base material showing a prepreg 20 according to a second embodiment.
[0084] Figure 4 The prepreg 20a shown contains a fiber substrate 4 in the second region 2a. In cross-sectional view, one surface S4α of the fiber substrate 4 is roughly consistent with one surface S2α of the second region 2a, and another surface S4β of the fiber substrate 4 is roughly consistent with another surface S2β of the second region 2a.
[0085] In other words, Figure 4 The prepreg 20a shown in the cross-section has: a composite layer 2a, which contains the thermosetting resin composition contained in the second region and the fiber substrate 4; and a resin layer 1a, which is located on both sides of the composite layer 2a, and contains the thermosetting resin composition contained in the first region, and does not contain the fiber substrate. The composite layer 2a corresponds to the second region, and the resin layer 1a corresponds to the first region.
[0086] Figure 5 The illustrated prepreg 20b contains a fiber substrate 4 in the second region 2b.
[0087] In the prepreg 20b, a surface S2α of the second region 2b on the one surface Sα side of the prepreg 20b exists closer to the one surface Sα of the prepreg 20b than a surface S4α of the fiber base material 4 on the one surface Sα side.
[0088] In the prepreg 20b, the surface S2β of the second region 2b on the other surface Sβ side of the prepreg 20b exists closer to the other surface Sβ of the prepreg 20b than the surface S4β of the fiber base material 4 on the other surface Sβ side.
[0089] In other words, Figure 5 The prepreg 20b shown has resin layers 1b containing the thermosetting resin composition contained in the first region and containing no fiber substrate on both sides of the composite layer 2b containing the thermosetting resin composition contained in the second region and the fiber substrate 4 in cross-sectional view.
[0090] The composite layer 2b corresponds to the second region, and the resin layer 1b corresponds to the first region.
[0091] Figure 6 and Figure 7 2 is a schematic cross-sectional view illustrating a fiber base material in a prepreg 30 according to a third embodiment.
[0092] Figure 6 The prepreg 30a shown contains a fiber substrate 4 in the third region 3a'. In cross-sectional view, one surface S4α of the fiber substrate 4 is roughly consistent with one surface S3α of the third region 3a', and another surface S4β of the fiber substrate 4 is roughly consistent with another surface S3β of the third region 3a'.
[0093] In other words, Figure 6 The prepreg 30a shown, when viewed in cross section, has, on both sides of a composite layer 3a' containing a third thermosetting resin composition and a fiber substrate 4, a second resin layer 2a' containing the thermosetting resin composition contained in the second region and not containing a fiber substrate, and a first resin layer 1a' containing the thermosetting resin composition contained in the first region and not containing a fiber substrate, starting from the surface of the composite layer 3a'.
[0094] The composite layer 3 a ′ corresponds to the third region, the first resin layer 1 a ′ corresponds to the first region, and the second resin layer 2 a ′ corresponds to the second region.
[0095] Figure 7The illustrated prepreg 30b includes a fiber base material 4 in the second region 2b' and the third region 3b'.
[0096] In the prepreg 30b, a surface S2α of the second region 2b′ on the one surface Sα side of the prepreg 30b exists closer to the one surface Sα of the prepreg 30b than a surface S4α of the fiber base material 4 on the one surface Sα side.
[0097] In the prepreg 30b, the surface S2β of the second region 2b' on the other surface Sβ side of the prepreg 30b exists closer to the other surface Sβ of the prepreg 30b than the surface S4β of the fiber base material 4 on the other surface Sβ side.
[0098] In other words, Figure 7 The prepreg 30b shown in the cross-section has, on both sides of the first composite layer 3b' containing the third thermosetting resin composition and the fiber substrate 4, a second composite layer 2b' containing the thermosetting resin composition contained in the second region and the fiber substrate, and a resin layer 1b' containing the thermosetting resin composition contained in the first region and not containing the fiber substrate, starting from the surface of the first composite layer 3b'.
[0099] The first composite layer 3 b ′ corresponds to the third region, the second composite layer 2 b ′ corresponds to the second region, and the resin layer 1 b ′ corresponds to the first region.
[0100] <Prepreg Thickness>
[0101] The thickness of the prepreg of the present embodiment is not particularly limited and may be appropriately determined depending on the intended use, but is preferably 20 to 200 μm, more preferably 30 to 150 μm, and still more preferably 40 to 100 μm.
[0102] <Storage modulus E' of cured prepreg at 40°C>
[0103] The storage modulus E' of the cured product of the prepreg of this embodiment at 40°C (hereinafter also referred to as "40°C storage modulus E'") is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 5 to 30 GPa, more preferably 8 to 20 GPa, and further preferably 10 to 15 GPa.
[0104] In addition, the 40° C. storage modulus E′ of the cured product of the prepreg can be measured by the method described in the Examples.
[0105] <Thickness of Each Region>
[0106] The thickness of the first region is not particularly limited, but is preferably 5 to 70 μm, more preferably 6 to 50 μm, and even more preferably 7 to 30 μm from the viewpoint of improving the warpage change amount of the semiconductor package and the conductor adhesion.
[0107] The thickness of the second region is not particularly limited, but is preferably 5 to 150 μm, more preferably 10 to 100 μm, and even more preferably 15 to 50 μm from the viewpoint of improving the warpage change amount of the semiconductor package and the conductor adhesion.
[0108] When the prepreg of this embodiment has a third region, the thickness of the third region is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 5 to 150 μm, more preferably 10 to 100 μm, and further preferably 15 to 50 μm.
[0109] The total volume occupied by the first region in the prepreg of the present embodiment is not particularly limited; however, from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 10 to 80% by volume, more preferably 20 to 70% by volume, and even more preferably 30 to 60% by volume relative to the total prepreg of the present embodiment.
[0110] The total volume occupied by the second region in the prepreg of this embodiment is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 20 to 90 volume %, more preferably 30 to 80 volume %, and further preferably 40 to 70 volume % relative to the total prepreg of this embodiment.
[0111] The total volume occupied by the first region and the second region in the prepreg of the present embodiment is not particularly limited, but is preferably 60 to 100% by volume, more preferably 80 to 100% by volume, and even more preferably 95 to 100% by volume relative to the entire prepreg of the present embodiment.
[0112] <Storage modulus of each thermosetting resin composition>
[0113] The 260°C storage modulus E'(1) of the cured product of the thermosetting resin composition contained in the first region is not particularly limited, but is preferably 0.1 to 1.5 GPa, more preferably 0.3 to 1.0 GPa, and even more preferably 0.5 to 0.7 GPa from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0114] The 260°C storage modulus E'(2) of the cured product of the thermosetting resin composition contained in the second region is not particularly limited, but is preferably 0.5 to 2.0 GPa, more preferably 0.8 to 1.3 GPa, and even more preferably 1.0 to 1.2 GPa from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0115] The difference [E'(2)-E'(1)] between the 260°C storage modulus E'(1) of the cured product of the thermosetting resin composition contained in the first region and the 260°C storage modulus E'(2) of the cured product of the thermosetting resin composition contained in the second region is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 0.05 to 1.5 GPa, more preferably 0.2 to 1.0 GPa, and even more preferably 0.4 to 0.6 GPa.
[0116] In addition, the 260° C. storage modulus E′ of the cured product of the thermosetting resin composition contained in the first region and the thermosetting resin composition contained in the second region can be measured by the method described in the Examples.
[0117] The 40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the first region is not particularly limited, but is preferably 2 to 10 GPa, more preferably 3 to 8 GPa, and even more preferably 4 to 6 GPa from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0118] The 40° C. storage modulus E′ of the cured product of the thermosetting resin composition contained in the second region is not particularly limited, but is preferably 3 to 12 GPa, more preferably 4 to 10 GPa, and even more preferably 5 to 7 GPa from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0119] The difference between the 40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the first region and the 40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the second region [40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the second region - 40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the first region] is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 0.1 to 5 GPa, more preferably 0.5 to 3 GPa, and even more preferably 0.8 to 1.5 GPa.
[0120] In addition, the 40° C. storage modulus E′ of the cured product of the thermosetting resin composition contained in the first region and the thermosetting resin composition contained in the second region can be measured by the method described in the Examples.
[0121] When the prepreg of this embodiment has a third region, the suitable ranges of the 260°C storage modulus E' and the 40°C storage modulus E' of the cured product of the third thermosetting resin composition are the same as the suitable ranges of the 260°C storage modulus E' and the 40°C storage modulus E' of the cured product of the thermosetting resin composition contained in the first region.
[0122] <Composition of Each Thermosetting Resin Composition>
[0123] The composition of each thermosetting resin composition is described below. It should be noted that in the following description, unless otherwise specified, when simply referred to as "thermosetting resin composition", it refers to the thermosetting resin composition contained in the first region, the thermosetting resin composition contained in the second region, and the third thermosetting resin composition contained as required.
[0124] The thermosetting resin composition contains at least a thermosetting resin.
[0125] The thermosetting resin composition preferably contains, in addition to the thermosetting resin, at least one selected from, for example, an inorganic filler, a curing agent, a curing accelerator, an organic filler, a coupling agent, a leveling agent, an antioxidant, a flame retardant, a flame retardant aid, a thixotropy imparting agent, a thickener, a flexible material, a surfactant and a photopolymerization initiator, and more preferably contains an inorganic filler and a curing accelerator.
[0126] Hereinafter, each component which the thermosetting resin composition may contain will be described.
[0127] In addition, each component may be used individually by 1 type, or may use 2 or more types together.
[0128] (Thermosetting resin)
[0129] Examples of thermosetting resins include epoxy resins, polyimide resins, maleimide resins, modified maleimide resins, phenolic resins, polyphenylene ether resins, bismaleimide triazine resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins.
[0130] Among them, maleimide resins, modified maleimide resins, epoxy resins, polyimide resins, cyanate resins, polyphenylene ether resins, and bismaleimide triazine resins are preferred from the viewpoints of moldability and electrical insulation, and maleimide resins, modified maleimide resins, and epoxy resins are more preferred.
[0131] The maleimide resin is preferably a maleimide resin having one or more N-substituted maleimide groups, and more preferably a maleimide resin having two or more N-substituted maleimide groups.
[0132] The maleimide resin is preferably an aromatic maleimide resin having an N-substituted maleimide group directly bonded to an aromatic ring.
[0133] Examples of maleimide resins include bis(4-maleimidephenyl)methane, bis(4-maleimidephenyl)ether, bis(4-maleimidephenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 4-methyl-1,3-phenylenebismaleimide, m-phenylenebismaleimide, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, and the like having two groups directly attached to an aromatic ring. Aromatic bismaleimide resins having bonded N-substituted maleimide groups; aromatic polymaleimide resins having three or more N-substituted maleimide groups directly bonded to aromatic rings, such as polyphenylmethane maleimide and biphenyl aralkyl maleimide; maleimide resins having an indane ring skeleton; aliphatic maleimide resins such as 1,6-bismaleimide-(2,2,4-trimethyl)hexane and pyrophosphate binder type long-chain alkyl bismaleimide, etc.
[0134] Examples of the modified maleimide resin include aminomaleimide resins having a structure derived from a maleimide resin and a structure derived from a diamine compound.
[0135] As the diamine compound, a compound having two primary amino groups is preferred.
[0136] Moreover, as a diamine compound, the aromatic diamine compound which has two primary amino groups directly bonded to an aromatic ring is preferable.
[0137] Examples of the diamine compound include aromatic diamines having two primary amino groups directly bonded to an aromatic ring, such as m-phenylenediamine, p-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(4-aminophenoxy)phenyl] sulfone, benzidine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl sulfide, and 4,4'-diamino-3,3'-biphenol; and siloxane compounds having two primary amino groups. Among them, 3,3'-dimethyl-4,4'-diaminodiphenylmethane and a siloxane compound having two primary amino groups are preferred.
[0138] As the siloxane compound having two primary amino groups, a siloxane compound having primary amino groups at both terminals is preferred, and a polydimethylsiloxane compound having primary amino groups at both terminals is more preferred.
[0139] The primary amino group equivalent of the siloxane compound having two primary amino groups is not particularly limited, but is preferably 300 to 2000 g / mol, more preferably 400 to 1500 g / mol, and further preferably 500 to 1000 g / mol.
[0140] The aminomaleimide resin may further have a structure derived from an amine compound having an acidic substituent, as necessary.
[0141] Examples of the amine compound having an acidic substituent include aminophenols such as o-aminophenol, m-aminophenol, and p-aminophenol; aminobenzoic acids such as p-aminobenzoic acid, m-aminobenzoic acid, and o-aminobenzoic acid; aminobenzenesulfonic acids such as o-aminobenzenesulfonic acid, m-aminobenzenesulfonic acid, and p-aminobenzenesulfonic acid; 3,5-dihydroxyaniline, 3,5-dicarboxyaniline, etc. Among them, aminophenol, aminobenzoic acid, and 3,5-dihydroxyaniline are preferred from the viewpoint of solubility and synthesis yield, and m-aminophenol and p-aminophenol are more preferred from the viewpoint of heat resistance.
[0142] The content of the structure derived from the maleimide resin in the aminomaleimide resin is not particularly limited, but is preferably 30 to 95% by mass, more preferably 50 to 90% by mass, and even more preferably 70 to 80% by mass.
[0143] The content of the structure derived from the diamine compound in the aminomaleimide resin is not particularly limited, but is preferably 2 to 50% by mass, more preferably 5 to 40% by mass, and further preferably 10 to 30% by mass.
[0144] The content of the structure derived from the amine compound having an acidic substituent in the aminomaleimide resin is not particularly limited, but is preferably 0.1 to 10% by mass, more preferably 0.5 to 7% by mass, and further preferably 1 to 5% by mass.
[0145] The aminomaleimide resin can be produced by reacting a maleimide resin, a diamine compound, and, if necessary, an amine compound having an acidic substituent by a known method.
[0146] The content of one or more selected from maleimide resins and modified maleimide resins in the thermosetting resin is not particularly limited, but is preferably 40 to 98% by mass, more preferably 60 to 95% by mass, and further preferably 70 to 90% by mass.
[0147] As the epoxy resin, an epoxy resin having two or more epoxy groups is preferred. The epoxy resin can be classified into glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among them, glycidyl ether type epoxy resin is preferred.
[0148] Epoxy resins can also be classified into various types of epoxy resins according to the differences in their main skeletons.
[0149] Specifically, epoxy resins can be classified into bisphenol epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin; bisphenol novolac epoxy resins such as bisphenol A novolac epoxy resin and bisphenol F novolac epoxy resin; novolac epoxy resins other than the above bisphenol novolac epoxy resins such as phenol novolac epoxy resin, cresol novolac epoxy resin, and biphenyl novolac epoxy resin; phenol aralkyl epoxy resins; stilbene epoxy resins; naphthalene Epoxy resins containing naphthalene skeletons such as phenol novolac epoxy resins, naphthol epoxy resins, naphthol aralkyl epoxy resins, and naphthylene ether epoxy resins; biphenyl epoxy resins; biphenyl aralkyl epoxy resins; xylylene epoxy resins; dihydroanthracene epoxy resins; alicyclic epoxy resins such as saturated dicyclopentadiene epoxy resins; heterocyclic epoxy resins; epoxy resins containing spiro rings; cyclohexanedimethanol epoxy resins; trimethylol epoxy resins; aliphatic chain epoxy resins; rubber-modified epoxy resins; etc. Among them, biphenyl aralkyl epoxy resins are preferred.
[0150] The content of the epoxy resin in the thermosetting resin is not particularly limited, but is preferably 2 to 60% by mass, more preferably 5 to 40% by mass, and further preferably 10 to 30% by mass.
[0151] The content of the thermosetting resin in the resin component contained in the thermosetting resin composition is not particularly limited, but from the viewpoints of heat resistance, conductor adhesion, etc., it is preferably 30 to 100% by mass, more preferably 50 to 100% by mass, and even more preferably 70 to 100% by mass relative to the total amount of the resin component in the thermosetting resin composition.
[0152] Here, in this specification, the "resin component" means a resin and a compound that forms a resin by a curing reaction.
[0153] The volume-based content of the resin component in the thermosetting resin composition contained in the first region is not particularly limited, but from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 40 to 95 volume %, more preferably 50 to 90 volume %, and further preferably 60 to 80 volume %.
[0154] The volume-based content of the resin component in the thermosetting resin composition contained in the second region is not particularly limited, but is preferably 20 to 80 volume %, more preferably 30 to 70 volume %, and further preferably 40 to 60 volume % from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0155] (Inorganic filler)
[0156] From the viewpoint of further improving the warpage change amount of the semiconductor package and the conductor adhesion, the thermosetting resin composition preferably contains an inorganic filler.
[0157] As inorganic fillers, for example, silica, alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, silicon carbide, etc. Among them, silica and alumina are preferred from the viewpoint of reducing the coefficient of thermal expansion, the relative dielectric constant and the dielectric loss tangent, and silica and aluminum hydroxide are preferred from the viewpoint of heat resistance.
[0158] The inorganic filler may be surface-treated with a surface treatment agent such as a silane coupling agent.
[0159] The average particle size of the inorganic filler (D 50) is not particularly limited, but from the viewpoint of dispersibility of the inorganic filler and fine wiring properties, it is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, and further preferably 0.2 to 1 μm.
[0160] It should be noted that the average particle size (D 50 ) is the particle size corresponding to the point of 50% volume when the cumulative frequency distribution curve based on the particle size is calculated with the total volume of the particles as 100%. The average particle size of the inorganic filler can be measured, for example, using a particle size distribution measuring device using a laser diffraction scattering method.
[0161] Examples of the shape of the inorganic filler include spherical shapes and crushed shapes, and a spherical shape is preferred.
[0162] Preferably, the thermosetting resin composition contained in the first region and the thermosetting resin composition contained in the second region contain an inorganic filler, and the volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region is lower than the volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region.
[0163] The volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region is not particularly limited, but is preferably 5 to 60 volume %, more preferably 10 to 50 volume %, and further preferably 20 to 40 volume % from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0164] The volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region is not particularly limited, but is preferably 20 to 80 volume %, more preferably 30 to 70 volume %, and further preferably 40 to 60 volume % from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion.
[0165] The difference (V(2)-V(1)) between the volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region and the volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region is not particularly limited; however, from the viewpoint of improving the warpage change of the semiconductor package and the conductor adhesion, it is preferably 2 to 40 volume %, more preferably 10 to 30 volume %, and even more preferably 15 to 25 volume %.
[0166] The third thermosetting resin composition may or may not contain an inorganic filler. When the inorganic filler is contained, the appropriate content thereof is the same as the range of the appropriate content of the inorganic filler in the thermosetting resin composition contained in the first region on a volume basis.
[0167] (Curing accelerator)
[0168] Examples of the curing accelerator include acidic catalysts such as p-toluenesulfonic acid; amine compounds such as triethylamine, tributylamine, pyridine, and dicyandiamide; imidazole compounds such as methylimidazole, phenylimidazole, 2-heptadecylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-phenylimidazolium trimellitate; isocyanate-blocked imidazole compounds such as an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole; quaternary ammonium compounds; phosphorus compounds such as triphenylphosphine; organic peroxides such as dicumyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butyl peroxyisopropyl monocarbonate, and α,α'-bis(tert-butylperoxy)diisopropylbenzene; carboxylates of manganese, cobalt, zinc, and the like; Among them, imidazole compounds are preferred from the viewpoint of the curing acceleration effect and storage stability.
[0169] When the thermosetting resin composition contains a curing accelerator, the content of the curing accelerator is not particularly limited, but is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the thermosetting resin, from the viewpoint of the curing acceleration effect and storage stability.
[0170] The solid content derived from the thermosetting resin composition in the prepreg of the present embodiment is not particularly limited, but is preferably 20 to 80% by mass, more preferably 25 to 70% by mass, and even more preferably 30 to 60% by mass.
[0171] <Fiber base material>
[0172] As the material of the fiber substrate, for example, natural fibers such as paper and cotton linters; inorganic fibers such as glass fibers and asbestos; organic fibers such as aramid, polyimide, polyvinyl alcohol, polyester, tetrafluoroethylene, acrylic fibers; mixtures thereof, etc. Among them, inorganic fibers are preferred, and glass fibers are more preferred from the viewpoint of flame retardancy.
[0173] Examples of the glass fiber include glass fibers made of E glass, C glass, D glass, S glass, and the like.
[0174] The material of the fiber base material may be one kind alone or two or more kinds may be combined.
[0175] Examples of the shape of the fiber substrate include woven fabric, nonwoven fabric, roving, chopped strand mat, and surface mat. Among these, woven fabric is preferred.
[0176] Among the above options, glass cloth is preferred as the fiber base material from the viewpoints of low thermal expansion, flame retardancy, versatility, and the like.
[0177] The fiber substrate may be a fiber substrate composed of one layer or a fiber substrate composed of multiple layers. It should be noted that the fiber substrate composed of one layer means a fiber substrate composed only of entangled fibers. If there is a fiber substrate that is not entangled, it is classified as a fiber substrate composed of multiple layers. The material and shape of the fiber substrates of two or more layers may be the same or different.
[0178] The thickness of the fiber substrate is not particularly limited and may be appropriately determined depending on the intended use. However, it is preferably 10 to 150 μm, more preferably 20 to 100 μm, and still more preferably 30 to 60 μm.
[0179] [Laminated board]
[0180] The laminated plate of the present embodiment is a laminated plate including a cured product of the prepreg of the present embodiment and a metal foil.
[0181] In addition, a laminated plate having a metal foil is sometimes also referred to as a metal-clad laminated plate.
[0182] The metal of the metal foil is not particularly limited, and examples thereof include copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, and alloys containing one or more of these metal elements.
[0183] The laminated plate of the present embodiment can be produced, for example, by placing a metal foil on one or both surfaces of the prepreg of the present embodiment and then performing heat-pressing molding.
[0184] Usually, the B-staged prepreg is cured by the heat and pressure molding to obtain the laminated plate of the present embodiment.
[0185] When performing heat and pressure molding, only one prepreg may be used, or two or more prepregs may be stacked. It should be noted that, when two or more prepregs are stacked, it is preferred that at least one surface of the insulating layer included in the obtained laminate is composed of the cured product of the first region.
[0186] For the heat and pressure molding, for example, a multistage press, a multistage vacuum press, a continuous molding machine, an autoclave molding machine, etc. can be used.
[0187] The conditions for heat and pressure molding are not particularly limited, but may be, for example, a temperature of 100 to 300° C., a time of 10 to 300 minutes, and a pressure of 1.5 to 5 MPa.
[0188] [Printed circuit board]
[0189] The printed wiring board of the present embodiment is a printed wiring board having a cured product of the prepreg of the present embodiment.
[0190] The printed wiring board of this embodiment can be manufactured by forming a conductor circuit on the cured product of the prepreg of this embodiment by a known method. It should be noted that the surface on which the conductor circuit is formed is preferably a surface formed by the cured product of the first region of the prepreg of this embodiment.
[0191] Furthermore, a multilayer printed wiring board can be manufactured by further performing a multilayer bonding process as needed. The conductor circuit can be formed by, for example, appropriately performing a hole forming process, a metal plating process, or etching of a metal foil.
[0192] [Semiconductor packaging]
[0193] The semiconductor package of the present embodiment is a semiconductor package including the printed wiring board of the present embodiment and a semiconductor element.
[0194] The semiconductor package of this embodiment can be manufactured, for example, by mounting a semiconductor element on a printed circuit board of this embodiment using a known method. It should be noted that the surface on which the semiconductor element is mounted is preferably a surface formed by a cured product of the first region of the prepreg of this embodiment or a surface on which a conductor circuit is formed.
[0195] Example
[0196] The present embodiment will be described in detail below with reference to examples, but the present embodiment is not limited to the following examples.
[0197] [Method for measuring storage modulus E' at 40°C and 260°C of cured product of thermosetting resin composition]
[0198] Copper foil was arranged on both sides of the resin film obtained in each example, and the resin film was cured by pressing for 85 minutes under the conditions of a pressure of 1.0 MPa and a maximum holding temperature of 240°C using a forming press to obtain a resin plate with copper foil on both sides. The obtained resin plate with copper foil on both sides was immersed in an etching solution to remove the copper foil on both sides, and was cut into 5 mm × 40 mm, and the obtained resin plate was set as a test piece. The test piece was used as a measurement object, and a dynamic viscoelasticity measuring device (manufactured by UBM Co., Ltd., trade name "Rheogel-E4000") was used to measure the storage modulus E' under the conditions of a measurement temperature range of 30 to 350°C, a heating rate of 5°C / min, and a frequency of 10Hz, and the storage modulus E' at 40°C and 260°C was obtained.
[0199] [Synthesis of modified maleimide resin]
[0200] Synthesis example 1
[0201] Into a 1L reaction vessel equipped with a thermometer, a stirrer and a reflux condenser capable of heating and cooling, 19.4 g of a polydimethylsiloxane compound having primary amino groups at both ends (Toray Dow Corning Co., Ltd., trade name "X-22-161A", primary amino group equivalent: 800 g / mol), 13.0 g of 3,3'-diethyl-4,4'-diaminodiphenylmethane, 122.9 g of 4,4'-bismaleimide diphenylmethane, 4.7 g of p-aminophenol, and 240.0 g of propylene glycol monomethyl ether were added, and after reacting at 115° C., the mixture was concentrated under normal pressure so that the resin concentration was 60% by mass. Subsequently, 53.3 g of cyclohexanone was added at 90° C. and stirred for 30 minutes to obtain a solution of a modified maleimide resin.
[0202] [Manufacture of resin varnish]
[0203] Production Example 1
[0204] (Resin varnish 1)
[0205] 300 parts by mass of the modified maleimide resin solution obtained in Synthesis Example 1, 170 parts by mass of spherical silica (average particle size (D 50 )0.25μm, surface treated with 3-aminopropyltrimethoxysilane), 1.2 parts by mass of 2-heptadecylimidazole (manufactured by Shikoku Chemicals Co., Ltd., trade name "C17Z"), and 65 parts by mass of biphenyl aralkyl linear phenolic epoxy resin (manufactured by Nippon Kayaku Co., Ltd., trade name "NC-3000-H") were mixed with methyl ethyl ketone, stirred and mixed at 25°C or while heated to 50-80°C, thereby preparing a resin varnish 1 with a solid content concentration of about 65% by mass.
[0206] The volume-based content of the spherical silica relative to the total solid content of the resin varnish 1 was 30% by volume.
[0207] Production Example 2
[0208] (Resin varnish 2)
[0209] A resin varnish 2 having a solid content concentration of about 65% by mass was prepared in the same manner as in Production Example 1 except that the blending amount of spherical silica was changed to 400 parts by mass.
[0210] The volume-based content of the spherical silica relative to the total solid content of the resin varnish 2 was 50% by volume.
[0211] [Manufacture of resin film, prepreg and copper-clad laminate]
[0212] Examples 1 to 3, Comparative Examples 1 to 3
[0213] (1) Preparation of resin film
[0214] The resin varnishes 1 and 2 obtained above were applied to one surface of a 50 μm thick PET film, respectively, and then dried by heating at 125° C. for 3 minutes to form a resin film composed of a thermosetting resin composition on the PET film, thereby obtaining a resin film with a PET film.
[0215] Hereinafter, the resin film formed of the resin varnish 1 is referred to as "low elastic resin film A", and the resin film formed of the resin varnish 2 is referred to as "high elastic resin film B". The low elastic resin film A and the high elastic resin film B were prepared to have thicknesses of 8 μm, 10 μm, and 12 μm, respectively.
[0216] (2) Bonding between resin films
[0217] The low elastic resin film A with PET film obtained above and the high elastic resin film B with PET film were overlapped so that the resin films were in contact with each other, and were laminated using a laminator while heating at 100° C. Similarly, the low elastic resin films A with PET film and the high elastic resin films B with PET film were laminated to each other, and six types of resin films with PET films on both sides having the following structures were obtained.
[0218] ■Resin film AB1 with PET films on both sides: has a laminated structure of PET film / low elastic resin film A (thickness 10 μm) / high elastic resin film B (thickness 10 μm) / PET film in this order.
[0219] ■Resin film AB2 with PET films on both sides: has a laminated structure of PET film / low elastic resin film A (thickness 8 μm) / high elastic resin film B (thickness 12 μm) / PET film in this order.
[0220] ■Resin film AB3 with PET films on both sides: has a laminated structure of PET film / low elastic resin film A (thickness 12 μm) / high elastic resin film B (thickness 8 μm) / PET film in this order.
[0221] ■Resin film AA with PET films on both sides: has a laminated structure of PET film / low elastic resin film A (thickness 10 μm) / low elastic resin film A (thickness 10 μm) / PET film in this order.
[0222] ■Resin film BB with PET films on both sides: has a laminated structure of PET film / highly elastic resin film B (thickness 10 μm) / highly elastic resin film B (thickness 10 μm) / PET film in this order.
[0223] (3) Preparation of prepreg
[0224] The resin film obtained above was Figure 8 As shown, the prepreg (thickness: 60 μm) was prepared by laminating the glass cloth in a manner of forming a structure of outer region (11) / inner region (21) / inner region (22) / outer region (12). The resin films used in forming each region are shown in Table 1. In addition, the specific production steps are shown below.
[0225] It should be noted that the thicknesses of the outer regions (11) and (12) and the inner regions (21) and (22) shown in Table 1 include the glass cloth when the region includes the glass cloth.
[0226] (Example 1)
[0227] Two films were prepared by peeling off the PET film on one side where the high elastic resin film B was exposed from the resin film AB 1 with PET films on both sides. Then, the two sides of the E glass cloth with a thickness of 0.04 mm were overlapped so that the exposed high elastic resin film B was in contact with the glass cloth, and laminated using a laminator while heating at 130° C., and the PET films on both sides were peeled off, thereby obtaining a prepreg. The solid content of the thermosetting resin composition in the obtained prepreg was 40% by mass.
[0228] (Example 2)
[0229] A prepreg was prepared in the same manner as in Example 1 except that the resin films laminated on both sides of the glass cloth were changed to resin film AB2 with PET films on both sides. The solid content derived from the thermosetting resin composition in the obtained prepreg was 39% by mass.
[0230] (Example 3)
[0231] A prepreg was prepared by the same procedure as in Example 1 except that the resin films laminated on both sides of the glass cloth were changed to resin film AB3 with PET films on both sides. The solid content derived from the thermosetting resin composition in the obtained prepreg was 41% by mass.
[0232] (Comparative Example 1)
[0233] A prepreg was prepared in the same manner as in Example 1 except that the resin films laminated on both sides of the glass cloth were changed to resin films BB with PET films on both sides. The solid content derived from the thermosetting resin composition in the obtained prepreg was 34% by mass.
[0234] (Comparative Example 2)
[0235] A prepreg was prepared in the same manner as in Example 1 except that the resin films laminated on both sides of the glass cloth were changed to resin films AA with PET films on both sides. The solid content derived from the thermosetting resin composition in the obtained prepreg was 47% by mass.
[0236] (Comparative Example 3)
[0237] Two films were prepared by peeling off the PET film on one side of the resin film AB 1 with PET films on both sides and removing the PET film exposed by the low elastic resin film A. Then, the two films were overlapped on both sides of the glass cloth so that the exposed low elastic resin film A was in contact with the glass cloth, and laminated under the same conditions as in Example 1, thereby preparing a prepreg. The solid content of the thermosetting resin composition in the obtained prepreg was 40% by mass.
[0238] (4) Fabrication of double-sided copper-clad laminates
[0239] Then, using the prepreg obtained in each example, a double-sided copper-clad laminate was produced.
[0240] Eight prepregs obtained in each example were stacked, and an electrolytic copper foil with a thickness of 12 μm was arranged so that the M surface was in contact with the prepreg. The stack was heated and pressed at a temperature of 240° C., a pressure of 3.0 MPa, and a time of 85 minutes to produce a double-sided copper-clad laminate (thickness: about 0.5 mm).
[0241] [Evaluation method]
[0242] The double-sided copper-clad laminate obtained in each example was used to perform various evaluations according to the following methods. The results are shown in Table 1.
[0243] (Method for measuring thermal expansion coefficient and glass transition temperature)
[0244] The copper foil on both sides of the double-sided copper-clad laminate obtained in each example was removed by etching to produce a 5 mm square evaluation substrate. Then, a thermomechanical analysis was performed using a thermomechanical measuring device (TMA) (manufactured by TA Instruments Japan Co., Ltd., trade name "Q400") using a compression method. After the evaluation substrate was installed in the above-mentioned device, it was continuously measured twice under the measurement condition of a heating temperature of 10°C / minute. It should be noted that the thermal expansion coefficient is the thermal expansion coefficient in the surface direction of the laminate, and the average thermal expansion coefficient in the temperature range of 25 to 120°C and the average thermal expansion coefficient of 250 to 280°C in the second measurement were obtained respectively.
[0245] (Method for measuring storage modulus E' at 40°C)
[0246] The copper foils on both sides of the double-sided copper-clad laminate obtained in each example were removed by etching, cut into 5 mm × 40 mm, and the obtained laminate was used as a test piece. The test piece was used as the measurement object, and the 40°C storage modulus E' was measured under the same conditions as the above [Measurement method of storage modulus E' of cured product of thermosetting resin composition].
[0247] (Method for measuring the peel strength of copper foil)
[0248] The copper foil of the double-sided copper-clad laminate obtained in each example was etched into a straight line with a width of 3 mm, and the obtained laminate was used as a test piece. The formed straight copper foil was installed in a small desktop tester (manufactured by Shimadzu Corporation, trade name "EZ-TEST"), and the copper foil peel strength was measured by pulling it in a 90° direction at room temperature (25°C). It should be noted that the pulling speed when pulling the copper foil was set to 50 mm / min.
[0249] (Measurement method of warpage change)
[0250] The copper foils on both sides of the double-sided copper-clad laminate obtained in each example were removed by etching, and the laminate was cut into 40 mm×40 mm to serve as a substrate.
[0251] A 25 mm × 25 mm silicon chip was placed in the center of one surface of the substrate, and a liquid sealing material (manufactured by Showa Denko Materials Co., Ltd., trade name "CEL-C-3730 series") was filled in the gap between the substrate and the silicon chip, and heated at 140°C for 3 hours to cure the liquid sealing material and seal. The substrate with the silicon chip thus obtained was used as a semiconductor package for measuring the warpage change.
[0252] The semiconductor package obtained above was used as the measurement object, and the warpage change amount due to temperature was measured by the shadow moiré method using a warpage measurement device with a heating mechanism, manufactured by AKROMETRIX, trade name "THERMOIRE PS200". Specifically, the test piece was heated from 25°C to 260°C and then naturally cooled to room temperature twice, and the absolute value of the difference between the warpage amount at 25°C and the warpage amount at 260°C in the second time was set as the warpage change amount.
[0253] [Table 1]
[0254] Table 1
[0255]
[0256] As shown in Table 1, the copper foil peel strength of the copper-clad laminate formed by the prepregs of Examples 1 to 3 of the present embodiment is high, and the warpage change of the semiconductor package using the copper-clad laminate is small. On the other hand, the warpage change of the semiconductor package using the copper-clad laminate formed by the prepregs of Comparative Examples 1 to 3 is large, and the copper foil peel strength of the copper-clad laminate formed by the prepregs of Comparative Examples 1 and 3 is low.
[0257] Description of Reference Numerals
[0258] 10, 20, 20a, 20b, 30, 30a, 30b prepreg, 1 first region, 2 second region, 3 third region, 4 fiber substrate, 1a resin layer (first region), 2a composite layer (second region), 1b resin layer (first region), 2b composite layer (second region), 1a' first resin layer (first region), 2a' second resin layer (second region), 3a' composite layer (third region), 1b' resin layer (first region), 2b' second composite layer (second region), 3b' first composite layer (third region), (11) outer region, (12) outer region, (21) inner region, (22) inner region, Sα, Sβ surface of prepreg, S2α, S2β surface of the second region, S3α, S3β surface of the third region, S4α, S4β surface of fiber substrate, X, X1, X2 directions.
Claims
1. A prepreg comprising a thermosetting resin composition and a fiber substrate, The prepreg has one surface and another surface on the opposite side to the one surface, The prepreg has, starting from at least one of the one surface and the other surface and in a surface direction opposite to the surface serving as the starting point, the following components, in order: a first region constituting the surface of the prepreg serving as the starting point and containing a thermosetting resin composition; and a second region containing a thermosetting resin composition different from the thermosetting resin composition contained in the first region, The storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region is lower than the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region.
2. The prepreg according to claim 1, wherein The prepreg has the first region and the second region in this order, with each of the one surface and the other surface as a starting point, in a surface direction opposite to the surface serving as the starting point.
3. The prepreg according to claim 1 or 2, wherein: The difference between the storage modulus E'(1) at 260°C of the cured product of the thermosetting resin composition contained in the first region and the storage modulus E'(2) at 260°C of the cured product of the thermosetting resin composition contained in the second region, i.e., E'(2)-E'(1), is 0.05 GPa to 1.5 GPa.
4. The prepreg according to claim 1 or 2, wherein The storage modulus E'(1) of the cured product of the thermosetting resin composition contained in the first region at 260° C. is 0.1 GPa to 1.5 GPa.
5. The prepreg according to claim 1 or 2, wherein: The storage modulus E'(2) of the cured product of the thermosetting resin composition contained in the second region at 260° C. is 0.5 GPa to 2.0 GPa.
6. The prepreg according to claim 1 or 2, wherein: The thermosetting resin composition contained in the first region and the thermosetting resin composition contained in the second region contain an inorganic filler. A volume-based content V(1) of the inorganic filler in the thermosetting resin composition in the first region is lower than a volume-based content V(2) of the inorganic filler in the thermosetting resin composition in the second region.
7. The prepreg according to claim 6, wherein The difference between the volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region and the volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region, i.e., V(2)-V(1), is 2 volume % to 40 volume %.
8. The prepreg according to claim 1 or 2, wherein: The volume-based content V(1) of the inorganic filler in the thermosetting resin composition contained in the first region is 5% by volume to 60% by volume.
9. The prepreg according to claim 1 or 2, wherein: The volume-based content V(2) of the inorganic filler in the thermosetting resin composition contained in the second region is 20% to 80% by volume. 10 . A laminate comprising a cured product of the prepreg according to claim 1 or 2 and a metal foil.
11. A printed wiring board comprising a cured product of the prepreg according to claim 1 or 2.