Method for manufacturing semiconductor device
Through the exposure and development technology of the positive photosensitive resin film, a mask is formed for plasma cutting, which solves the fragmentation problem caused by laser groove processing and improves the quality of the semiconductor chip.
Patent Information
- Application Number
- CN202480002315.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-28
- Publication Date
- 2024-12-06
AI Technical Summary
During the plasma cutting process, laser groove processing causes fine chips to remain on the sides of the semiconductor chip, affecting the chip quality.
A positive photosensitive resin film is used for exposure and development, and a pattern is formed as a mask for plasma cutting, avoiding laser groove processing, thereby suppressing the generation of debris.
Without laser groove processing, the pattern is successfully formed and the generation of fragments is suppressed, thereby improving the quality of the semiconductor chip.
Smart Images

Figure CN119096329A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art
[0002] Semiconductor devices are usually manufactured through the following steps. First, a semiconductor wafer is attached to a dicing tape and the semiconductor wafer is singulated into semiconductor chips in this state (dicing step). After that, a pickup step of picking up the semiconductor chip and a semiconductor chip bonding step of bonding the picked-up semiconductor chip and a supporting member by thermal compression bonding via an adhesive (die bonding film) are performed, thereby manufacturing a semiconductor device.
[0003] As one of the dicing methods in the dicing step, there is known a method of performing plasma etching (dry etching) along the planned cutting line of the semiconductor wafer to cut the semiconductor wafer. The process of processing the semiconductor wafer by this dicing method is called plasma dicing.
[0004] In plasma cutting, a protective film is usually formed on the surface of a semiconductor wafer, and a portion of the protective film is removed by irradiating a laser along a predetermined cutting line to burn off the protective film (laser grooving process), thereby forming a pattern (mask) from the protective film. In the laser grooving process, fine shavings (debris) are generated from the protective film, the semiconductor wafer, etc., and the debris remains on the side of the obtained semiconductor chip, which sometimes reduces the quality of the semiconductor chip. In Patent Document 1, research was conducted on suppressing the residue of debris in plasma cutting.
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2019-050237 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] An object of the present invention is to provide a novel method for manufacturing a semiconductor device including a step of performing plasma dicing.
[0010] Means for solving technical problems
[0011] The present invention provides a method for manufacturing a semiconductor device according to [1] to [3].
[0012] [1] A method for manufacturing a semiconductor device, comprising:
[0013] A step of forming a positive photosensitive resin film on the surface of a semiconductor wafer;
[0014] exposing a portion of the positive photosensitive resin film to light and providing an exposure portion on the positive photosensitive resin film;
[0015] A step of developing the positive photosensitive resin film using a developer and removing the exposed portion to form a pattern;
[0016] A step of singulating the semiconductor wafer by performing plasma dicing using the pattern as a mask to obtain semiconductor chips with the pattern;
[0017] A process of exposing the pattern of the patterned semiconductor chip; and
[0018] A step of removing the exposed pattern using a removing liquid to obtain a semiconductor chip in which the pattern is removed from the semiconductor chip with the pattern.
[0019] [2] The method for manufacturing a semiconductor device according to [1], wherein:
[0020] The positive photosensitive resin composition includes a resin whose molecular weight is reduced by irradiation with light.
[0021] [3] The method for manufacturing a semiconductor device according to [2], wherein the developer and the remover are aqueous solvents having a pH of 11 or less.
[0022] Effects of the Invention
[0023] According to the present invention, a novel method for manufacturing a semiconductor device including a step of performing plasma dicing is provided. According to the method for manufacturing a semiconductor device of the present invention, a pattern (mask) can be formed without performing laser grooving processing, and generation of debris itself can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 1 middle, Figure 1 (a) Figure 1 (b) Figure 1 (c), and Figure 1 (d) is a diagram showing each process.
[0025] Figure 2 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 2 middle, Figure 2 (a) Figure 2 (b) Figure 2 (c) Figure 2 (d) and Figure 2 (e) is a diagram showing each process. DETAILED DESCRIPTION
[0026] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including steps, etc.) are not necessary unless otherwise specified. The same symbols are marked on the same or equivalent parts, and repeated descriptions are omitted. In addition, the positional relationships such as up, down, left, and right are assumed to be based on the positional relationships shown in the accompanying drawings unless otherwise specified. The sizes of the constituent elements in each figure are conceptual, and the relative relationship between the sizes of the constituent elements is not limited to the relationship shown in each figure.
[0027] The same is true for the numerical values and their ranges in the present invention, and the present invention is not limited thereto. In this specification, the numerical range shown by "~" is used to represent the range in which the numerical values before and after "~" are included as the minimum value and the maximum value, respectively. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Moreover, in the numerical ranges recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiments.
[0028] In this specification, the term "layer" includes not only structures having shapes formed on the entire surface but also structures having shapes formed on a portion of the surface when viewed from a top view. In this specification, the term "process" includes not only independent processes but also processes that cannot be clearly distinguished from other processes as long as the desired effect of the process can be achieved.
[0029] In the present specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acrylic copolymers.
[0030] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0031] [Method for manufacturing semiconductor device]
[0032] The method for manufacturing a semiconductor device of the present embodiment comprises: a step of forming a positive photosensitive resin film on the surface of a semiconductor wafer (hereinafter sometimes referred to as “step (A)”); a step of exposing a portion of the positive photosensitive resin film and providing an exposure portion on the positive photosensitive resin film (hereinafter sometimes referred to as “step (B)”); a step of developing the positive photosensitive resin film with a developer and removing the exposure portion to form a pattern (hereinafter sometimes referred to as “step (C)”); a step of singulating the semiconductor wafer by plasma dicing using the pattern as a mask to obtain a semiconductor chip with a pattern (hereinafter sometimes referred to as “step (D)”); a step of exposing the pattern of the semiconductor chip with a pattern (hereinafter sometimes referred to as “step (E)”); and a step of removing the exposed pattern with a removing solution to obtain a semiconductor chip with the pattern removed from the semiconductor chip with a pattern (hereinafter sometimes referred to as “step (F)”). Figure 1 and Figure 2 This is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device.
[0033] <Process (A)>
[0034] In this step, a positive photosensitive resin film 4 is formed on the surface of the semiconductor wafer 1 .
[0035] The positive photosensitive resin film 4 is a resin film in which the exposed portion whose solubility is increased is removed by treatment with a developer, and the unexposed portion remains. The positive photosensitive resin film 4 may include, for example, a known positive photoresist material.
[0036] The positive photosensitive resin film 4 may include a resin that is reduced in molecular weight by irradiation with light (hereinafter, sometimes referred to as a "photofusible resin"). The photofusible resin may be a resin having properties such as reduced in molecular weight by irradiation with light, thereby reducing the elastic modulus and increasing the loss tangent (tanδ). The photofusible resin may be a water-insoluble resin, and may be a resin having properties such as reduced in molecular weight by irradiation with light, thereby imparting a water-soluble gel or liquid (increased solubility in an aqueous solvent).
[0037] In one embodiment, the photofusible resin may be a reaction product of a compound A having a disulfide bond and having two or more thiol groups and a compound B having two or more functional groups capable of reacting with the thiol groups. The positive photosensitive resin film 4 may further include a photoradical generator in addition to the photofusible resin. The positive photosensitive resin film 4 may further include a curing accelerator that promotes the reaction of the compound A and the compound B.
[0038] The mechanism of the photofusible resin being reduced in molecular weight (melting) is not always obvious, but for example, the following mechanism can be considered. However, it is not limited to these mechanisms. The photofusible resin contains a compound having a disulfide bond (a reaction product of compound A and compound B). By irradiating the photofusible resin contained in the positive photosensitive resin film 4 with light, the disulfide bonds in the photofusible resin are decomposed (cleaved) and thiol radicals are generated. At this time, if there is a photoradical generator (intramolecular cleavage type photoradical generator), the thiol radical reacts with the photoradical generator, and the thiol radical is capped by the photoradical generator. Therefore, it can be considered that the compound having a disulfide bond is reduced in molecular weight and the cured product is photosoftened (photomelted). As another mechanism, it can also be considered that the photoinduced radicals generated by the photoradical generator (intramolecular cleavage type photoradical generator) directly react with the disulfide bond, resulting in the formation of a photoinduced radical-thioether bond and the generation of a thiol radical, and the thiol radical reacts with another photoinduced radical to lower the molecular weight of the compound having a disulfide bond itself, thereby softening the photocured material. It can be said that the reaction of disulfide bond cleavage is an irreversible reaction.
[0039] The positive photosensitive resin film 4 containing a photofusible resin can be formed, for example, by disposing a curable composition containing compound A, compound B, a photo radical generator and a curing accelerator as required on the surface of a semiconductor wafer 1, and curing the curable composition by heating or light irradiation (reacting compound A and compound B). At this time, the positive photosensitive resin film 4 can include a cured product of the curable composition. The cured product of the curable composition can include a reaction product of compound A and compound B and a photo radical generator. Here, the curable composition can be a thermosetting composition cured by heating, or a photocurable composition cured by light irradiation, preferably a thermosetting composition. Below, each component of the curable composition is described.
[0040] (Compound A)
[0041] Compound A is a compound having a disulfide bond (-SS-) and having two or more thiol groups (-SH). The upper limit of the number of thiol groups of compound A may be, for example, 10 or less, 8 or less, 6 or less, or 4 or less. Component (A) may be, for example, a dithiol compound, which is a compound having two thiol groups (-SH). Component (A) may be a high molecular weight component of a polymer or oligomer. A compound having two thiol groups (-SH) may be considered to be a compound formed by two thiol groups and a group (the first connecting group) that includes a disulfide bond and connects the two thiol groups.
[0042] The molecular weight or number average molecular weight of compound A may be, for example, 100 to 10,000,000, 200 to 3,000,000, 300 to 1,000,000, 400 to 10,000, or 500 to 5,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0043] Compound A has one or more (two or more) disulfide bonds in the molecule. The number of disulfide bonds in Compound A may be, for example, 1 to 1000 or 4 to 50.
[0044] Compound A may be a compound (e.g., a polymer or oligomer) having a linear or branched molecular chain and an end group, and having a disulfide bond in the molecular chain. In this case, the end group in compound A may be a thiol group. By including such a compound as compound A in the curable composition, there is a tendency to further improve the optical melting property of the optically melting resin (the reaction product of compound A and compound B). The molecular chain in compound A may contain a disulfide bond and a polyether chain, or may be formed by a disulfide bond and a polyether chain.
[0045] Compound A can be, for example, a compound represented by formula (1): HS-(XSS) n1 -X-SH (compound (1)). In the formula, X represents a polyether chain. Multiple Xs may be the same or different. n1 represents an integer greater than 1. n1 may be, for example, 1 or more or 4 or more, and may be 1000 or less. In the case where component (A) is a compound represented by formula (1), -(XSS) n1 The group represented by -X- is the first linking group. The compound for extending the chain of compound (1) may be, for example, a Michael adduct of compound (1) or a thiocarbamate of compound (1).
[0046] The polyether chain as X may be, for example, a polyoxyalkylene chain. The polyether chain as X may be, for example, a 1 -OX 2 -OX 3 - represents a group. 1 ~X 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 2 carbon atoms (for example, methylene group, ethylene group). As for the polyether chain as X, for example, -CH2CH2-O-CH2-O-CH2CH2- and the like can be mentioned.
[0047] As commercially available products of compound A, for example, THIOKOL LP series (dithiol having a disulfide bond, manufactured by TORAY FINE CHEMICALS CO., LTD.) and the like can be cited. Compound A can be obtained by converting the reactive functional group of a compound having a reactive functional group (e.g., carboxyl group, hydroxyl group) and a disulfide bond at the terminal into a thiol group. As compounds having a reactive functional group and a disulfide bond at the terminal, 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol, cystamine and the like can be cited.
[0048] The content of compound A may be 15 mass % or more, 25 mass % or more, or 35 mass % or more, and 80 mass % or less, 70 mass % or less, or 60 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0049] (Compound B)
[0050] Compound B is a compound having two or more functional groups capable of reacting with a thiol group. As a functional group capable of reacting with a thiol group, for example, a cyclic ether group (ethylene oxide (oxiranyl, epoxy), oxetane group (oxetanyl group), tetrahydrofuranyl, tetrahydropyranyl, etc.); isocyanate group; ethylenically unsaturated group (C=C), etc. The upper limit of the number of functional groups of compound B can be, for example, 10 or less, 8 or less, 6 or less, or 4 or less.
[0051] Compound B may be compound B1 having a polyether chain and having two or more cyclic ether groups. Since the curable composition contains compound B1 as compound B, the low molecular weight components generated by irradiating the photofusible resin with light have a large number of polyether chains or hydroxyl groups and tend to be water-soluble, and thus the low molecular weight components can be removed with an aqueous solvent.
[0052] From the viewpoint of reactivity and availability, the cyclic ether group can be an ethylene oxide group. That is, compound B1 is an ethylene oxide compound (epoxy compound) having a polyether chain and having more than 2 ethylene oxide groups (oxiranyl, epoxy group). In addition, in this specification, in the cyclic ether group, a group having a cyclic ether structure (a structure comprising a cyclic ether group) is included. For example, in the ethylene oxide group, a group having an ethylene oxide structure (a structure comprising an ethylene oxide (oxiranyl, epoxy group)) such as a glycidyl group, a glycidyl ether group, an epoxycyclohexyl group, etc. is included.
[0053] The molecular weight or number average molecular weight of compound B1 may be, for example, 100 to 1,000,000, 100 to 500,000, 100 to 10,000, 150 to 5,000, or 200 to 2,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0054] When the cyclic ether group of compound B1 is an oxyethylene group (oxiranyl group, epoxy group), the epoxy equivalent of component (B) may be 50 to 2000 g / eq, 80 to 1500 g / eq, or 100 to 1000 g / eq.
[0055] Compound B1 may be a compound B1a having two cyclic ether groups, or a compound B1b having three or more cyclic ether groups. Compound B1a may be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. In this case, the end group in compound B1a may be a cyclic ether group. Compound B1a can be regarded as a compound formed by two cyclic ether groups and a group (the second connecting group) comprising a polyether chain and connecting the two cyclic ether groups. Compound B1b may be a compound having one or more cyclic ether groups as a side chain or substituent of the second connecting group in compound B1a. From the viewpoint of being able to further shorten the curing time and being able to further improve the optical solubility and water solubility, compound B1 may include both compound B1a and compound B1b.
[0056] Compound B1a may be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. In this case, the end group in compound B1a may be a cyclic ether group. In the case where compound B is compound B1a, there is a tendency to easily remove low molecular components generated by irradiating light to the photofusible resin with an aqueous solvent. The polyether chain as a molecular chain may have a hydroxyl group, an alkyl group having a hydroxyl group, or other substituents. The molecular chain in compound B1a may include a polyether chain or may be formed by a polyether chain.
[0057] Compound B1a can be, for example, a compound represented by formula (2): Z-(Y) n2 -Z represents a compound (compound (2)). In the formula, Y represents a polyether chain, and Z represents a cyclic ether group. Multiple Zs may be the same or different. n2 represents an integer greater than 1. n2 may be, for example, greater than 1 or greater than 2, and may be less than 1000. In the case where compound B1a is compound (2), -(Y) n2 The group represented by - is the second connecting group.
[0058] The polyether chain as Y may be, for example, a polyoxyalkylene chain. The polyether chain as Y may be, for example, a 1 -OY 2 -OY 3 -represented by a group. 1 ~Y 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 3 carbon atoms (for example, methylene, ethylene, propylene). As for the polyether chain as Y, for example, -CH2CH2-O-CH2-CH2-O-CH2CH2- and the like can be mentioned.
[0059] Examples of commercially available products of compound B1a include DENACOL EX series (EX-850, EX-851, EX-821, EX-830, EX-832, EX-841, EX-861, EX-920, manufactured by Nagase ChemteX Corporation).
[0060] Compound B1b may be a compound having one or more cyclic ether groups as side chains of the second linking group (polyether chain as Y) in compound B1a.
[0061] Examples of commercially available products of compound B1b include DENACOL EX series (EX-614B, EX-313, EX-512, EX-521, manufactured by Nagase ChemteX Corporation).
[0062] The mass ratio of the content of compound B1b to the total content of compound B1a and compound B1b (content (mass) of compound B1b / total content (mass) of compound B1a and compound B1b) may be 0.01 to 0.40. If the mass ratio is 0.01 or more, there is a tendency that the curing time of the curable composition can be further shortened, and if the mass ratio is 0.40 or less, there is a tendency that the optical melting property and water solubility can be further improved. The mass ratio may be 0.02 or more or 0.03 or more, and may be 0.35 or less, 0.30 or less, 0.25 or less, 0.20 or less, 0.15 or less, or 0.10 or less.
[0063] The content of compound B may be 10 mass % or more, 20 mass % or more, or 30 mass % or more, and 60 mass % or less, 50 mass % or less, or 40 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0064] The ratio of the total number of moles of thiol groups in compound A to the total number of moles of functional groups in compound B may be, for example, 0.90 or more or 0.95 or more, and 1.10 or less or 1.05 or less.
[0065] (Photoradical Generator)
[0066] The photoradical generator is a component that generates free radicals by light irradiation. For example, the photoradical generator can use a component used as a photopolymerization initiator. As the photoradical generator, there can be mentioned an intramolecular cleavage type photoradical polymerization initiator in which the photoradical generator itself is photocleaved by light irradiation to generate two free radicals.
[0067] Examples of the intramolecular cleavage type photoradical generator include benzyl ketal photoradical generators, α-aminoalkylphenone photoradical generators, α-hydroxyalkylphenone photoradical generators, α-hydroxyacetophenone photoradical generators, and acylphosphine oxide photoradical generators.
[0068] Examples of the benzyl ketal-based photoradical generator include 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad 651) and the like.
[0069] Examples of α-aminoalkylphenone-based photoradical generators include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (Omnirad369), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (Omnirad907), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (Omnirad379EG).
[0070] Examples of the α-hydroxyalkylphenone-based photoradical generator include 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184) and the like.
[0071] Examples of the α-hydroxyacetophenone-based photoradical generator include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propane-1-one (Omnirad127) and 2-hydroxy-2-methyl-1-phenyl-propane-1-one (Omnirad1173).
[0072] Examples of the acylphosphine oxide-based photoradical generator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO H) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819).
[0073] The content of the photoradical generator may be 1 mass % or more, 3 mass % or more, or 5 mass % or more, and may be 30 mass % or less, 20 mass % or less, or 15 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0074] From the viewpoint of further improving photosensitivity, the ratio of the mole number of the photoradical generator to the mole number of compound A (mole number of photoradical generator / mole number of compound A) may be 0.1 or more, 0.2 or more, or 0.3 or more.
[0075] (Curing accelerator)
[0076] The curing accelerator is a component for accelerating the reaction between compound A and compound B, and includes a component that functions as a catalyst for the curing reaction (catalyst-type curing agent). Examples of the curing accelerator include amine compounds, imidazole derivatives, quaternary ammonium salts, organic metal salts, phosphorus compounds, and the like.
[0077] Examples of the amine compound include dicyandiamide, trimethylamine, triethylamine, tripropylamine, tributylamine, tri-n-octylamine, dimethylethylamine, dimethylpropylamine, dimethylbutylamine, dimethyl-n-octylamine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, benzyldimethylamine, 4-methyl-N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine.
[0078] Examples of the imidazole derivatives include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole, 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4,5-triphenylimidazole, 1-benzyl-2-imidazole, 1,2-dimethylimidazole, and 1-benzyl-2-phenylimidazole.
[0079] Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetraethylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltributylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrabutylammonium bromide, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrabutylammonium iodide, and benzyltributylammonium iodide.
[0080] Examples of the organic metal salt include organic metal salts such as bis(2,4-pentanedione)zinc(II), zinc octylate, zinc naphthenate, cobalt naphthenate, copper naphthenate, iron acetylacetonate, nickel octylate, and manganese octylate.
[0081] Examples of the phosphorus compound include tetraphenylphosphoniumtetra-p-tolylborate, tetraphenylphosphoniumtetra-p-tolylborate, triphenylphosphine, tri-p-tolylphosphine, tri(4-chlorophenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(2,6-dimethoxyphenyl)phosphine, triphenylphosphinetriphenylborane, tetraphenylphosphonium dicyanamide, and tetraphenylphosphoniumtetra(4-methylphenyl)borate.
[0082] The content of the curing accelerator may be 0.01 mass %, 0.1 mass % or 0.5 mass % or more, and may be 10 mass %, 5 mass % or less, or 2 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0083] The curable composition may further include components (other components) that do not belong to compound A, compound B, a photoradical generator, and a curing accelerator. As other components, for example, plasticizers, adhesiveness imparting agents such as tackifiers, antioxidants, colorless dyes, sensitizers, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, defoamers, fillers, chain transfer agents, thixotropy imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents and other additives can be used for these additives. Known additives can be used. In the case where the curable composition includes other components, the total amount of the content of the other components is based on the total amount of the curable composition, and can be 0 to 95% by mass, 0.01 to 50% by mass, or 0.1 to 10% by mass.
[0084] The curable composition can be used as a varnish of the curable composition diluted with a solvent. As the solvent, for example, aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-isopropylbenzene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides (NMP) such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. The content of the solid content in the varnish, that is, the content other than the solvent in the varnish, can be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.
[0085] Step (A) includes, for example, a step of preparing a stacked body 10 including a dicing tape 2 (dicing film) and semiconductor wafers 1 placed on the dicing tape 2 (see Figure 1and the positive photoresist material is disposed on the surface of the semiconductor wafer 1, forming a positive photosensitive resin film 4 step (reference Figure 1 (b)).
[0086] When the positive photosensitive resin film 4 includes a photofusible resin, the step (A) includes, for example, a step of preparing the laminate 10 (see Figure 1 (a)); a step of configuring a curable composition on the surface of the semiconductor wafer 1; and a step of curing the curable composition to form a positive photosensitive resin film 4 comprising a cured product of the curable composition (reference Figure 1 (b)).
[0087] Examples of the semiconductor wafer 1 include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide. The semiconductor wafer 1 may include electrodes such as through electrodes.
[0088] The thickness of the semiconductor wafer 1 may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.
[0089] As the dicing tape 2 (dicing film), for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. In addition, the dicing tape can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape can also have adhesiveness. This dicing tape can impart adhesiveness to the above-mentioned plastic film, and can also be provided with a pressure-sensitive adhesive layer on one surface of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be formed by a UV-curable pressure-sensitive adhesive or a non-UV-curable pressure-sensitive adhesive. There is no particular limitation on the UV-curable pressure-sensitive adhesive or the non-UV-curable pressure-sensitive adhesive as long as it has sufficient adhesive strength to prevent the semiconductor chips from flying around during the dicing process, and any conventionally known ones can be used.
[0090] The thickness of the dicing tape 2 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 300 μm.
[0091] The laminated body 10 can be obtained by bonding the semiconductor wafer 1 to the surface to which the adhesiveness of the dicing tape 2 is imparted or the surface provided with the pressure-sensitive adhesive layer.
[0092] The laminated body 10 may further include a dicing ring 3 disposed on the dicing tape 2 so as to surround the semiconductor wafer 1. The dicing ring 3 is a ring-shaped jig for fixing the semiconductor wafer 1 in the dicing step.
[0093] The curable composition can be prepared, for example, by a method including the step of mixing or kneading the above-mentioned components. The mixing and kneading can be carried out by appropriately combining a common disperser such as a stirrer, a pestle, a three-roll mill, a ball mill, or a bead mill.
[0094] There are no particular restrictions on the method of configuring the curable composition on the surface of the semiconductor wafer, but for example, there can be mentioned a method of applying the curable composition on the surface of the semiconductor wafer 1 using a spin coater, a bar coater, etc., and a method of forming the curable composition into a film and attaching the formed curable composition film to the semiconductor wafer 1 (transfer). The curable composition film may be in a semi-cured state (B stage state) before the curable composition film is attached to the semiconductor wafer 1. The curable composition can be configured on the circuit formation surface of the semiconductor wafer 1, for example.
[0095] About the solidified material of curable composition, for example, it can be obtained by heating curable composition. By heating curable composition, the reaction of compound A and compound B is carried out. At this time, curing accelerator can promote the reaction. The reaction product (light-melting resin) of compound A and compound B can be, for example, a compound (polymer) having a structure represented by the following formula. On the other hand, the participation of light free radical generator in the reaction is small, and the solidified material of curable composition can include the reaction product (light-melting resin) of compound A and compound B and light free radical generator.
[0096]
[0097] In the formula, X represents the first linking group, and Y represents the second linking group. m represents an integer greater than 1. For example, m may be greater than 50, greater than 100, greater than 500, or greater than 1000. * represents a bonding hand.
[0098] The heating temperature of the curable composition may be, for example, 0 to 200° C., 30 to 150° C., or 60 to 100° C. The heating time of the curable composition may be, for example, 0.1 to 168 hours, or 72 hours or less, 48 hours or less, or 24 hours or less.
[0099] The positive photosensitive resin film 4 may be in a (completely) cured state (C-stage state). The thickness of the positive photosensitive resin film 4 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 200 μm.
[0100] In this manner, the positive photosensitive resin film 4 containing the photofusible resin can be formed on the surface of the semiconductor wafer 1 .
[0101] <Process (B)>
[0102] In this step, a part of the positive photosensitive resin film 4 is exposed, and an exposure portion 4 a is provided on the positive photosensitive resin film 4 .
[0103] The exposure is performed on the positive photosensitive resin film 4, for example, along the planned cutting line of the semiconductor wafer 1. Thus, the positive photosensitive resin film 4 can be provided with an exposed portion 4a where the exposure is performed and an unexposed portion 4b where the exposure is not performed (see FIG. Figure 1 (c)).
[0104] There are no particular restrictions on the irradiation device and irradiation light used for performing the exposure, as long as the exposure portion 4a and the unexposed portion 4b can be provided. The exposure can be performed, for example, by irradiating the laser light A using the laser irradiation device 5. By using the laser irradiation device 5, the laser light A can be selectively irradiated to the desired portion of the positive photosensitive resin film 4 along the planned cutting line of the semiconductor wafer 1, and the exposure portion 4a and the unexposed portion 4b can be provided.
[0105] The laser light A irradiated to the positive photosensitive resin film 4 may be, for example, ultraviolet light or visible light. When the positive photosensitive resin film 4 includes a photofusible resin, the wavelength of the laser light A may be arbitrarily set, for example, according to the type of the photoradical generator used. The wavelength of the laser light A may be, for example, 150 to 550 nm.
[0106] As the laser irradiation device 5 , for example, a laser marking device, a laser scribing device, a focusing type irradiation device, etc. can be used.
[0107] As other methods of exposure, there can be mentioned a method of performing exposure via a mask or a reticle using an exposure device as implemented in a conventional photolithography method. As the exposure device, a contact aligner, a mirror projection, a stepper exposure device, etc. can be used. As the light source, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a halogen lamp, etc. can be mentioned.
[0108] <Process (C)>
[0109] In this step, the positive photosensitive resin film 4 is developed using a developer, and the exposed portion 4 a is removed to form a pattern 6 .
[0110] The developer used for development may be an aqueous solvent containing an alkaline compound such as sodium hydroxide, potassium hydroxide, sodium bicarbonate, sodium carbonate, sodium silicate, tetramethylammonium hydroxide, or an organic amine.
[0111] Examples of the aqueous solvent include water, a mixed solvent of water and a hydrophilic organic solvent, etc. In the mixed solvent of water and a hydrophilic organic solvent, the proportion of water can be, for example, 80% by mass or more. The aqueous solvent may contain additives such as a pH adjuster, a detergent, and a surfactant.
[0112] The aqueous solvent can be water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water, ultrapure water (Milli-Q water, etc.) etc. can be enumerated. In addition, Milli-Q water refers to the ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). Consider from the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water or ultrapure water.
[0113] Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.
[0114] As the pH adjusting agent, inorganic acids, inorganic bases, organic acids, organic bases, etc. can be mentioned. As inorganic acids, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, boric acid, etc. can be mentioned. As inorganic bases, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be mentioned. As organic acids, formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, picolinic acid, etc. can be mentioned. As organic bases, primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, imidazole compounds, etc. can be mentioned.
[0115] In the case where the positive photosensitive resin film 4 contains a photofusible resin, the developer used for development can be an aqueous solvent with a pH of less than 11. In addition, pH refers to the hydrogen ion index. The low molecular weight components generated by irradiating the photofusible resin with light have more polyether chains or hydroxyl groups and tend to be water-soluble. Therefore, the low molecular weight components can be removed with a weakly alkaline aqueous solvent or an aqueous solvent that does not contain an alkaline compound. In addition, by using an aqueous solvent with a pH of less than 11 as a developer, it is possible to suppress the chip scattering caused by the reduction in the adhesion of the dicing tape 2 to the semiconductor wafer 1, the developer penetrating the back of the chip, the embrittlement of the dicing tape 2, the expansion of the dicing tape 2, the defects in the assembly after the next process, the corrosion of the dicing ring 3, and other undesirable conditions. The pH of the aqueous solvent can be less than pH 10, less than pH 9, or less than pH 8, and can be greater than pH 4, greater than pH 5, or greater than pH 6.
[0116] The positive photosensitive resin film 4 is developed with a developer (the exposed portion 4a is removed with the developer), and the unexposed portion 4b remains on the semiconductor wafer 1, thereby forming a pattern 6. In this way, a laminated body 20 including a dicing tape 2, a semiconductor wafer 1 placed on the dicing tape 2, and a pattern 6 formed on the semiconductor wafer 1 can be obtained (see FIG. 1 ). Figure 1 (d)).
[0117] <Process (D)>
[0118] In this step, plasma dicing is performed using the pattern 6 as a mask to separate the semiconductor wafer 1 into pieces, thereby obtaining patterned semiconductor chips 8 .
[0119] The plasma used in plasma cutting is generated in the plasma generating device 7 under conditions such as being able to etch the semiconductor wafer 1. The etching conditions can be appropriately selected according to the material of the semiconductor wafer 1. When the material of the semiconductor wafer 1 is silicon, etching can be performed using the Bosch process. In the Bosch process, by sequentially repeating a protective film forming step, a protective film etching (anisotropic etching) step, and a Si etching (isotropic etching) step, etching is performed in the depth direction in a portion S on the surface of the semiconductor wafer 1 that is not covered by the pattern 6 (mask) (refer to Figure 2 (a)).
[0120] In the protective film forming step, for example, C4F8 or the like is supplied as a raw material gas in the plasma generating device 7, and the plasma is adjusted to a medium vacuum (10 -1 ~10 2 Pa), thereby generating plasma. Thus, a protective film can be formed on the Si surface, etc.
[0121] In the protective film etching step, for example, SF6 or the like is supplied as a raw material gas in the plasma generating device 7, and the medium vacuum (10 -1 ~10 2 Pa), thereby generating plasma. This enables etching of the protective film on the Si surface.
[0122] In the Si etching process, for example, SF6 or the like is supplied as a raw material gas in the plasma generating device 7, and the plasma is adjusted to a medium vacuum (10 -1 ~10 2 Pa), thereby generating plasma. Thus, the Si surface can be etched.
[0123] In this manner, a stacked body 30 including a dicing tape 2 and a plurality of patterned semiconductor chips 8 having semiconductor chips 1a and patterns 6 disposed on the dicing tape 2 can be obtained (see Figure 2 (b)).
[0124] <Process (E)>
[0125] In this step, the pattern 6 of the patterned semiconductor chip 8 is exposed.
[0126] Exposure is performed on pattern 6 (reference Figure 2 (c)). This can increase the solubility of the pattern 6 in a removing liquid to be described later.
[0127] The light B irradiating the pattern 6 may be ultraviolet light or visible light. When the positive photosensitive resin film 4 includes a photofusible resin, the wavelength of the light B may be appropriately selected according to the type of photoradical generator used. The wavelength of the light B may be, for example, 150 to 550 nm.
[0128] Regarding the irradiation of the light B, for example, the light irradiation device 9 can be used, and the irradiation amount can be set to 1000 mJ / cm 2 The irradiation dose can be appropriately set according to the wavelength of the light B, for example. The irradiation dose can be, for example, 3000 mJ / cm 2 Above, 5000mJ / cm 2 Above or 10000mJ / cm 2 Above, and can be 100000mJ / cm 2 Below, 80000mJ / cm 2 Below or 60000mJ / cm 2 the following.
[0129] The irradiation amount is the product of the illuminance and the irradiation time (seconds). Examples of light sources for irradiation with ultraviolet light or visible light include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, and LED lamps.
[0130] <Process (F)>
[0131] In this step, the exposed pattern 6 is removed using a removing liquid, thereby obtaining a semiconductor chip 1 a in which the pattern 6 is removed from the semiconductor chip 8 with a pattern.
[0132] As a removing liquid for removing the pattern 6, the same liquid as the developing liquid can be exemplified. The removing liquid may be an aqueous solvent containing an alkaline compound, and when the positive photosensitive resin film 4 contains a photofusible resin, it may be an aqueous solvent having a pH of 11 or less. The pH of the aqueous solvent may be pH 10 or less, pH 9 or less, or pH 8 or less, and may be pH 4 or more, pH 5 or more, or pH 6 or more.
[0133] In the conventional method for manufacturing a semiconductor device having a plasma dicing step, high pressure cleaning, ashing, and the like are sometimes performed when removing a pattern (mask). Since the method for removing the pattern 6 of the present embodiment does not perform high pressure cleaning, ashing, and the like, it can be said to be a simpler method than the conventional method. By removing the pattern 6, a stacked body 40 having a dicing tape 2 and a plurality of semiconductor chips 1a disposed on the dicing tape 2 can be obtained (see Figure 2 (d)).
[0134] The manufacturing method of the semiconductor device of the present embodiment may further include the following steps: a step of irradiating the pressure-sensitive adhesive layer of the dicing tape with ultraviolet rays (hereinafter, sometimes referred to as "step (G)"); a step of picking up the semiconductor chip (hereinafter, sometimes referred to as "step (H)"); a step of bonding the picked-up semiconductor chip and the supporting component by thermal compression bonding via an adhesive layer (grain bonding film, etc.) (hereinafter, sometimes referred to as "step (I)"); a thermal curing step of thermally curing the adhesive layer (hereinafter, sometimes referred to as "step (J)"), etc.
[0135] <Process (G)>
[0136] When the pressure-sensitive adhesive layer of the dicing tape 2 is composed of an ultraviolet curing pressure-sensitive adhesive, the method for manufacturing a semiconductor device may include a step (G). In this step, the pressure-sensitive adhesive layer is irradiated with ultraviolet rays. In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.
[0137] <Process (H)>
[0138] In this step, the individualized semiconductor chips 1 a are separated from each other, and the semiconductor chips 1 a lifted up from the dicing tape 2 by the ejector pins are sucked in by a suction chuck and picked up from the dicing tape 2 .
[0139] The ultraviolet irradiation step and the picking-up step may be performed after the step (E) and the step (F), or may be performed before the step (E) and the step (F).
[0140] <Step (I)>
[0141] In this step, the picked-up semiconductor chip 1a and the support member 11 are bonded by thermocompression through an adhesive layer 12 (die bonding film, etc.). The die bonding film used in this field can be used. A plurality of semiconductor chips 1a can be bonded to the support member 11.
[0142] The heating temperature during the thermocompression bonding may be, for example, 80 to 160° C. The load during the thermocompression bonding may be, for example, 5 to 15 N. The heating time during the thermocompression bonding may be, for example, 0.5 to 20 seconds.
[0143] <Process (J)>
[0144] In this step, the adhesive layer 12 is thermally cured. The heating temperature can be appropriately changed according to the constituent components of the die bonding film. The heating temperature can be, for example, 60 to 200° C., 90 to 190° C., or 120 to 180° C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. In addition, the temperature or pressure can be changed in stages for implementation.
[0145] In this manner, a semiconductor device 100 including a semiconductor chip 1a, a support member 11 on which the semiconductor chip 1a is mounted, and an adhesive layer 12 provided between the semiconductor chip 1a and the support member 11 to bond the semiconductor chip 1a and the support member 11 can be manufactured (see Figure 2 (e)).
[0146] According to the present invention, a novel method for manufacturing a semiconductor device including a step of performing plasma dicing is provided. According to the method for manufacturing a semiconductor device of the present invention, a pattern (mask) can be formed without performing laser grooving processing, and generation of debris itself can be suppressed.
[0147] Explanation of symbols
[0148] 1 semiconductor wafer, 1a semiconductor chip, 2 dicing tape, 3 dicing ring, 4 positive photosensitive resin film, 4a exposure portion, 4b unexposed portion, 5 laser irradiation device, 6 pattern (mask), 7 plasma generating device, 8 semiconductor chip with pattern, 9 light irradiation device, 10, 20, 30, 40 laminated body, 11 supporting member, 12 adhesive layer, 100 semiconductor device.
Claims
1. A method for manufacturing a semiconductor device, comprising: A step of forming a positive photosensitive resin film on the surface of a semiconductor wafer; exposing a portion of the positive photosensitive resin film to light and providing an exposure portion on the positive photosensitive resin film; A step of developing the positive photosensitive resin film using a developer and removing the exposed portion to form a pattern; A step of singulating the semiconductor wafer by performing plasma dicing using the pattern as a mask to obtain semiconductor chips with the pattern; A step of exposing the pattern of the patterned semiconductor chip; and A step of removing the exposed pattern using a removing liquid to obtain a semiconductor chip in which the pattern is removed from the semiconductor chip with the pattern.
2. The method for manufacturing a semiconductor device according to claim 1, wherein: The positive photosensitive resin film includes a resin whose molecular weight is reduced by irradiation with light.
3. The method for manufacturing a semiconductor device according to claim 2, wherein: The developer and the remover are aqueous solvents having a pH of 11 or less.
Citation Information