Ultraviolet cut-off adhesive film and solar cell

By using the ultraviolet cutoff film of bis-ethylhexyloxyphenol methoxyphenyltriazine and AB glue in perovskite solar cells, the perovskite solar cells are solved under ultraviolet conditions such as ultraviolet rays. The degradation problem improves the stability and service life of the battery.

CN222024285UActive Publication Date: 2024-11-19WUXI UTMOST LIGHT TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202323503501.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-11-19
Estimated Expiration
2033-12-20

AI Technical Summary

Technical Problem

Perovskite solar cells will irreversible degradation under conditions such as ultraviolet rays, moisture, and oxygen, resulting in reduced or failed battery efficiency, affecting their stability and industrial development.

Method used

A UV cutoff film is used, which contains bis-ethylhexyloxyphenol methoxyphenyl triazine as the ultraviolet absorbing layer, combined with transparent AB glue as the protective layer, effectively absorbing and blocking ultraviolet light and preventing it from penetrated to Inside the solar cell.

Benefits of technology

It significantly reduces the transmittance of ultraviolet light, improves the stability and service life of perovskite solar cells, slows down efficiency attenuation, and ensures the efficient performance of the battery in long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222024285U_ABST
    Figure CN222024285U_ABST
Patent Text Reader

Abstract

The utility model provides an ultraviolet cut-off adhesive film and a perovskite solar cell. The ultraviolet cut-off adhesive film comprises an ultraviolet light absorption layer, wherein the ultraviolet light absorption layer comprises bis-ethyl hexyloxyphenol methoxyphenyl triazine. Bis-ethylhexyloxyphenol methoxyphenyl triazine (BEMT) starts intramolecular excited state photon transfer after illumination, and after absorbed photon energy is converted into heat energy in a vibration relaxation mode to be released, the Bis-ethylhexyloxyphenol methoxyphenyl triazine quickly returns to a ground state, and the ultraviolet absorption capacity is recovered again, so that the ultraviolet absorption capacity of the Bis-ethylhexyloxyphenol methoxyphenyl triazine is improved. The bis-ethyl hexyloxyphenol methoxyphenyl triazine has very excellent ultraviolet absorption capability and light stability, so that the ultraviolet cut-off adhesive film disclosed by the utility model has long-term ultraviolet absorption capability and excellent light stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of solar cells, in particular to an ultraviolet cut-off adhesive film and a solar cell. Background Art

[0002] At present, the world is facing a serious energy shortage problem. Solar energy is an inexhaustible, clean and renewable energy source. Therefore, the efficient use of solar energy has become a trend in the development of new energy.

[0003] Perovskite solar cells are a new type of solar cell with simple process, extremely low cost and high photoelectric efficiency. At present, the photoelectric conversion efficiency of single-junction perovskite solar cells has reached 26.1%, showing great development potential in energy conversion. However, perovskite solar cells use an organic-inorganic hybrid perovskite material as a light-absorbing layer. This material will be severely degraded under conditions such as ultraviolet rays, moisture, and oxygen, and this degradation is irreversible, which will directly lead to reduced battery efficiency or even battery failure. Therefore, the stability of perovskite solar cells is a problem that must be solved for their industrial development. Utility Model Content

[0004] The utility model aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one purpose of the utility model is to provide a UV cut-off adhesive film, which can absorb UV light well and greatly reduce the transmittance of UV light.

[0005] In one aspect of the utility model, the utility model provides a UV cut-off adhesive film. According to an embodiment of the utility model, the UV cut-off adhesive film includes: an ultraviolet light absorbing layer, and the ultraviolet light absorbing layer includes bis-ethylhexyloxyphenol methoxyphenyl triazine. Bis-ethylhexyloxyphenol methoxyphenyl triazine (BEMT) initiates intramolecular excited state photon transfer after light irradiation, converts the absorbed photon energy into heat energy by vibrational relaxation, and then quickly returns to the ground state and restores the ultraviolet absorption ability. Therefore, bis-ethylhexyloxyphenol methoxyphenyl triazine (BEMT) has very excellent ultraviolet absorption ability and light stability, thereby making the ultraviolet cut-off adhesive film of the utility model have long-term ultraviolet absorption ability and excellent light stability.

[0006] According to an embodiment of the utility model, the UV cut-off film further includes: a protective layer, wherein the protective layer is arranged on one side of the UV light absorbing layer, and the side of the protective layer away from the UV light absorbing layer is a light receiving surface.

[0007] According to an embodiment of the utility model, the thickness of the ultraviolet light absorbing layer is 500 nanometers to 1 micrometer.

[0008] According to an embodiment of the utility model, the thickness of the protective layer is 0.5 to 1 mm.

[0009] According to an embodiment of the utility model, the protective layer is transparent glue.

[0010] According to an embodiment of the utility model, the transparent adhesive is an AB adhesive layer.

[0011] In another aspect of the utility model, the utility model provides a solar cell. According to an embodiment of the utility model, the solar cell includes the aforementioned UV cut-off adhesive film. Thus, the UV cut-off adhesive film can effectively absorb ultraviolet light, block ultraviolet light from irradiating the interior of the solar cell, reduce the amount of ultraviolet light incident on the solar cell, avoid ultraviolet light damage to the solar cell, slow down the efficiency decay of the perovskite solar cell, and thus improve the stability and service life of the solar cell.

[0012] According to an embodiment of the utility model, the solar cell is a perovskite solar cell, and the perovskite solar cell includes: a substrate, the substrate having a first surface and a second surface arranged opposite to each other; a perovskite cell chip, the perovskite cell chip is arranged on one side of the first surface; the ultraviolet light absorbing layer in the ultraviolet cutoff adhesive film is arranged on one side of the second surface.

[0013] According to an embodiment of the present invention, the UV cut-off adhesive film further includes a protective layer, and the protective layer is arranged on a side of the UV light absorbing layer away from the substrate.

[0014] According to an embodiment of the utility model, the perovskite battery chip includes: a first electrode layer, which is arranged on a side close to the first surface; a first charge transport layer, which is arranged on a side of the first electrode layer away from the substrate; a perovskite light absorption layer, which is arranged on a side of the first charge transport layer away from the substrate; a second charge transport layer, which is arranged on a side of the perovskite light absorption layer away from the substrate; and a second electrode layer, which is arranged on a side of the second charge transport layer away from the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0016] Figure 1 It is a schematic diagram of the structure of the UV cut-off adhesive film in one embodiment of the utility model;

[0017] Figure 2 It is a schematic structural diagram of a UV cutoff adhesive film in another embodiment of the utility model;

[0018] Figure 3 This is a schematic structural diagram of a perovskite solar cell in another embodiment of the present invention;

[0019] Figure 4 This is a schematic structural diagram of a perovskite solar cell in another embodiment of the present invention;

[0020] Figure 5 is a graph showing the attenuation of the efficiency of the perovskite solar cell during the light aging process in Examples 1 and 2 and Comparative Examples 1 and 2;

[0021] Figure 6 It is the light transmittance curve of the four-layer stacked structure of the UV cutoff film, substrate, first electrode layer and hole transport layer in Example 1, and the light transmittance curve of the three-layer stacked structure of the substrate, first electrode layer and hole transport layer in Test Comparative Example 1.

[0022] Figure numerals: 10 - UV cutoff film, 11 - UV light absorbing layer, 12 - protective layer, 30 - perovskite battery chip, 31 - first electrode layer, 32 - first charge transport layer, 33 - perovskite light absorbing layer, 34 - second charge transport layer, 35 - second electrode layer. DETAILED DESCRIPTION

[0023] The scheme of the utility model will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the utility model and should not be considered as limiting the scope of the utility model. Where specific techniques or conditions are not indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used are not indicated by the manufacturer and are all conventional products that can be obtained commercially.

[0024] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0025] In one aspect of the present invention, the present invention provides a UV cut-off adhesive film. According to an embodiment of the present invention, referring to Figure 1The UV cut-off adhesive film 10 includes: an UV light absorbing layer 11, and the UV light absorbing layer 11 includes bis-ethylhexyloxyphenol methoxyphenyl triazine. Bis-ethylhexyloxyphenol methoxyphenyl triazine (BEMT) initiates intramolecular excited state photon transfer after light irradiation, converts the absorbed photon energy into heat energy by vibration relaxation, and then quickly returns to the ground state and recovers the UV absorption ability. Therefore, bis-ethylhexyloxyphenol methoxyphenyl triazine has very excellent UV absorption ability and light stability, so that the UV cut-off adhesive film of the utility model has long-term UV absorption ability and excellent light stability; moreover, the UV light absorbing layer of the above material also has good transmittance to visible light.

[0026] In some embodiments of the present invention, the material of the ultraviolet light absorbing layer 11 is bis-ethylhexyloxyphenol methoxyphenyl triazine. In other words, the ultraviolet light absorbing layer 11 is composed of bis-ethylhexyloxyphenol methoxyphenyl triazine. Therefore, the ultraviolet light absorbing layer has excellent ultraviolet absorption ability.

[0027] According to some embodiments of the present invention, the thickness of the ultraviolet light absorbing layer 11 is 500 nanometers to 1 micrometer, for example, the thickness of the ultraviolet light absorbing layer 11 is 500 nanometers, 550 nanometers, 600 nanometers, 650 nanometers, 700 nanometers, 750 nanometers, 800 nanometers, 850 nanometers, 900 nanometers, 950 nanometers, 1000 nanometers (i.e., 1 micrometer), etc. The above thickness can make the ultraviolet light absorbing layer have good ultraviolet absorption ability, block the passage of ultraviolet light, and ensure the good transmittance of the ultraviolet light absorbing layer to visible light; if the thickness is relatively low, the ultraviolet absorption effect of the ultraviolet light absorbing layer will be relatively reduced; if the thickness is relatively thick, its transmittance to visible light will be relatively reduced.

[0028] According to some embodiments of the present invention, referring to Figure 2 The UV cut-off film 10 further includes: a protective layer 12, which is disposed on one side of the UV light absorbing layer 11, and the side of the protective layer 12 away from the UV light absorbing layer 11 is a light receiving surface, that is, light enters the UV cut-off film from one side of the protective layer. Thus, the UV cut-off film can be effectively protected from damage to the UV light absorbing layer by factors such as oxygen and water vapor in the external environment by the protective layer, thereby improving the stability and service life of the UV cut-off film, so that it can maintain a high absorption capacity for ultraviolet light for a long time. In some specific embodiments, the protective layer 12 is disposed on the surface of one side of the UV light absorbing layer 11.

[0029] According to some embodiments of the present invention, the thickness of the protective layer 12 is 0.5-1 mm, for example, the thickness of the protective layer is 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, etc. Therefore, the protective layer of the above thickness can effectively reduce the intrusion of external water vapor, and thus can well protect the ultraviolet light absorbing layer.

[0030] In some embodiments, the protective glue is a transparent glue, so that the protective layer has a good transmittance to visible light, so as to ensure the good visible light transmittance of the UV cutoff adhesive film as a whole. According to some embodiments of the utility model, the protective layer is an AB glue layer. As a protective layer, the AB glue not only has a better light transmittance to visible light, but also can well prevent the water and oxygen in the external environment from damaging the UV light absorbing layer. Furthermore, the AB glue can be well bonded to the surface of the UV light absorbing layer, improve the bonding force between the protective layer and the UV light absorbing layer, and thus improve the overall structural stability of the UV cutoff adhesive film. In this way, cracking between the protective layer and the UV light absorbing layer can be avoided during long-term use. If cracking occurs, water and oxygen in the external environment will penetrate into the UV light absorbing layer 11, thereby damaging it.

[0031] In some embodiments, in AB glue (two-component adhesive), A is the glue and B is the hardener. There are no special requirements for the specific type of AB glue, and those skilled in the art can flexibly select the raw material composition of AB glue in the prior art according to actual needs. In some embodiments, the mixing ratio of the glue A and the hardener B can be 1:1. Furthermore, the glue A can be an acrylic modified epoxy resin, and the hardener B can be a modified amine or other hardeners.

[0032] According to some embodiments of the present invention, the transmittance of the UV cutoff film 10 in the visible light band is greater than or equal to 95%. In this way, the UV cutoff film can effectively prevent the transmission of ultraviolet light without affecting the transmission of visible light, that is, the UV cutoff film not only has excellent absorption capacity for ultraviolet light, but also has good transmittance for visible light. In some embodiments of the present invention, the transmittance of the above-mentioned UV cutoff film to ultraviolet light is less than or equal to 1%, and can even reach a transmittance of 0%.

[0033] Among them, in some embodiments, the transmittance of the UV cut-off adhesive film 10 in the visible light band can be controlled by controlling the thickness of the UV light absorbing layer and the thickness of the protective layer. The smaller the thickness, the higher the transmittance of visible light, and the relatively worse the cut-off effect of UV light. The larger the thickness, the smaller the transmittance of visible light, and the relatively better the cut-off effect of UV light. In the present invention, the thickness of the UV light absorbing layer and the thickness of the protective layer can simultaneously achieve effective blocking of UV light and better transmittance of visible light.

[0034] According to some embodiments of the present invention, a method for preparing a UV cutoff film may include:

[0035] S100: Dissolve BEMT (bis-ethylhexyloxyphenol methoxyphenyl triazine) in a solvent, and stir to dissolve to obtain a certain concentration of ultraviolet absorption solution. In some embodiments, the solvent can be ethyl acetate (EA), chlorobenzene, ether and other solvents, and the concentration of bis-ethylhexyloxyphenol methoxyphenyl triazine in the ultraviolet absorption solution can be 100-200 mg / ml, so that it is easy to prepare an ultraviolet absorption layer of suitable thickness.

[0036] S200: Clean the surface of the substrate (e.g., the substrate in the perovskite solar cell), and then apply (e.g., by spin coating) the ultraviolet absorption solution obtained in S100 on the light-receiving surface of the substrate. In some embodiments, the specific cleaning method may be to use a cleaning agent (e.g., a glass cleaning agent) for cleaning, and then use ultraviolet ozone for surface treatment. In some embodiments, during the coating process of the ultraviolet absorption solution, the solvent in the ultraviolet absorption solution gradually evaporates, so that the ultraviolet absorption solution gradually forms a film to obtain a BEMT thin film.

[0037] S300: Evenly cover the AB glue on the surface of the spin-coated BEMT film, and obtain the protective glue after curing, thereby obtaining a UV cutoff glue film. In some embodiments, the curing temperature can be 50 to 80° C. (such as 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., etc.), and the curing time is 20 to 60 minutes.

[0038] It can be seen that the preparation method of the UV cutoff adhesive film of the utility model is simple and easy to implement, and has a high yield, and can be convenient for industrial mass production.

[0039] In another aspect of the utility model, the utility model provides a solar cell. According to an embodiment of the utility model, the solar cell includes the aforementioned UV cut-off adhesive film. Thus, the UV cut-off adhesive film can effectively absorb ultraviolet light, block ultraviolet light from irradiating the interior of the solar cell, reduce the amount of ultraviolet light incident on the solar cell, avoid ultraviolet light damage to the solar cell, and thus improve the stability and service life of the solar cell, slow down the efficiency decay of the solar cell, and improve the photoelectric conversion efficiency of the solar cell.

[0040] According to an embodiment of the present invention, the solar cell is a perovskite solar cell, referring to Figure 3The perovskite solar cell comprises: a substrate 20, the substrate 20 has a first surface 21 and a second surface 22 arranged opposite to each other; a perovskite light absorbing layer 30, the perovskite cell chip 30 is arranged on one side of the first surface 21; and the ultraviolet light absorbing layer 11 in the ultraviolet cut-off adhesive film 10 is arranged on one side of the second surface 22. The perovskite cell chip can refer to the general term for the film layer directly involved in the photoelectric conversion or charge transfer in the perovskite cell, which can generally include a perovskite light absorbing layer, a charge transfer layer, and an electrode layer. In the perovskite solar cell, light is incident from one side of the substrate 20, and the ultraviolet cut-off adhesive film 10 is arranged on the light receiving surface of the light. Before the light is incident on the inside of the solar cell, the ultraviolet light can be first absorbed, thereby reducing the ultraviolet incident amount of the solar cell, avoiding damage to the solar cell by ultraviolet light, and will not block the incident of visible light. In this way, the stability and service life of the perovskite solar cell can be effectively improved, and the photoelectric conversion efficiency of the perovskite solar cell can be improved.

[0041] There is no special requirement for the specific type of the substrate, and those skilled in the art can flexibly select according to actual needs. In some embodiments, the substrate is a flexible substrate, such as a PI (polyimide) substrate; in other embodiments, the substrate is a rigid substrate, such as a glass substrate.

[0042] According to some embodiments of the present invention, referring to Figure 4 The UV cut-off film 10 further includes a protective layer 12, which is disposed on the side of the UV light absorbing layer 11 away from the substrate 20. Thus, the UV light absorbing layer can be effectively protected from damage by factors such as oxygen and water vapor in the external environment by the protective layer, thereby improving the stability and service life of the UV cut-off film, so that it can maintain a high absorption capacity for UV light for a long time, and further slow down the efficiency decay of the perovskite solar cell.

[0043] According to some embodiments of the present invention, referring to Figure 3 and Figure 4 The perovskite battery chip 30 includes: a first electrode layer 31, which is arranged on a side close to the first surface 21; a first charge transport layer 32, which is arranged on a side of the first electrode layer 31 away from the substrate 20; a perovskite light absorption layer 33, which is arranged on a side of the first charge transport layer 32 away from the substrate 20; a second charge transport layer 34, which is arranged on a side of the perovskite light absorption layer 33 away from the substrate 20; and a second electrode layer 35, which is arranged on a side of the second charge transport layer 34 away from the substrate 10. Thus, the working efficiency of the perovskite solar cell can be improved.

[0044] Among them, the first charge transport layer and the second charge transport layer are transport layers for transporting different types of charges. In some embodiments, the first charge transport layer is an electron transport layer, and the second charge transport layer is a hole transport layer; in other embodiments, the first charge transport layer is a hole transport layer, and the second charge transport layer is an electron transport layer.

[0045] In some embodiments, there are no special requirements for the specific preparation methods, forming materials, and thickness of each layer structure of the above-mentioned structures such as the substrate 20, the first electrode layer 31, the first charge transport layer 32, the perovskite light absorption layer 33, the second charge transport layer 34, and the second electrode layer 35. Those skilled in the art can flexibly choose according to actual needs and existing technical means, and no further details will be given here.

[0046] According to some embodiments of the utility model, as shown above, the transmittance of the UV cut-off film 10 in the visible light band is greater than or equal to 95%, and the transmittance of the UV light is less than or equal to 1%, and can even reach a transmittance of 0%. It can be seen that the UV cut-off film of the utility model can maintain the long-term light stability of the battery without significantly reducing the battery efficiency, and can still maintain good battery efficiency during the long-term use of the perovskite solar cell.

[0047] According to some embodiments of the utility model, the specific application of the perovskite solar cell has no special requirements and can be used in a variety of electrical devices, such as wearable devices, smart phones, car batteries and other consumer electronics fields. In the industrial field, the perovskite solar cell of the utility model can also be used in photovoltaic power generation and other aspects.

[0048] According to some embodiments of the present invention, the method for preparing the perovskite solar cell may include:

[0049] T100 : preparing a first electrode layer 31 on the first surface of the substrate 20 .

[0050] In some embodiments, the first electrode layer is a FTO electrode, which can be prepared by evaporation, spin coating, spraying and other processes.

[0051] T200: preparing a first charge transport layer 32 on a side of the first electrode layer away from the substrate.

[0052] T300: coating a perovskite precursor solution on the side of the first charge transport layer 32 away from the substrate 20, and then performing an annealing treatment to obtain a perovskite light absorption layer 33. In some specific embodiments, the annealing temperature may be 110° C., and the annealing time may be 30 min.

[0053] T400: Evaporation of C on the side of the perovskite light absorbing layer 33 away from the substrate 20 60 / SnO2, to prepare the second charge transport layer 34.

[0054] T500: Evaporating a second electrode layer 35 on a side of the second charge transport layer 34 away from the substrate 20 to obtain a battery body. In some embodiments, the material of the second electrode layer can be copper.

[0055] T600: Evenly spread butyl rubber around the battery body and use white glass to cover the battery surface for packaging.

[0056] T700: On the light-receiving surface of the substrate 20 (ie, the surface of the substrate 20 away from the perovskite light-absorbing layer), prepare a UV cutoff film according to steps S100 to S200 or steps S100 to S400.

[0057] Example

[0058] Example 1

[0059] The structure of a perovskite solar cell is as follows Figure 3 As shown, the UV cut-off film only includes a UV light absorbing layer and does not include a protective layer, wherein the first charge transport layer 32 is a hole transport layer, and the second charge transport layer 34 is an electron transport layer.

[0060] Example 2

[0061] The structure of a perovskite solar cell is as follows Figure 4 As shown, the UV cut-off adhesive film includes a UV light absorbing layer and an AB adhesive layer stacked together, wherein the first charge transport layer 32 is a hole transport layer, and the second charge transport layer 34 is an electron transport layer.

[0062] Comparative Example 1

[0063] The difference from the first embodiment is that no UV cutoff film is provided on the light-receiving surface of the substrate 20 .

[0064] Comparative Example 2

[0065] The difference from the first embodiment is that instead of disposing an ultraviolet cut-off film on the light-receiving surface of the substrate 20 , a blue light quantum dot film is disposed on the light-receiving surface of the substrate 20 .

[0066] The perovskite solar cells in Examples 1 and 2 and Comparative Examples 1 and 2 were respectively subjected to current-voltage tests under a standard sunlight to obtain their short-circuit current densities (J sc ), open circuit voltage (V oc ), fill factor (FF) and photoelectric conversion efficiency (PCE), and then package it and perform light aging to test its efficiency change (i.e., efficiency attenuation). The test results are shown in Tables 1 and Figure 5 Among them, the calculation method of efficiency attenuation is:

[0067] 1. Efficiency change after encapsulation (aging 0 hours): (efficiency after encapsulation - efficiency before encapsulation) / efficiency before encapsulation × 100%. If the efficiency attenuation after encapsulation is within 5%, it means that the encapsulation process will not affect the efficiency of the component.

[0068] 2. Efficiency attenuation value after aging (120h, 220h, 390h, 720h) = (efficiency after aging - efficiency after packaging) / efficiency after packaging × 100%,

[0069] Among them, "unpackaged" refers to the efficiency tested before the implementation step of "evenly spreading butyl rubber around the battery body, covering the battery surface with white glass, and packaging".

[0070] Table 1

[0071]

[0072]

[0073] By comparing Example 1 with Comparative Example 1 and Comparative Example 2, it can be seen that by setting an ultraviolet light absorbing layer on the light-receiving surface of the battery, the damage of ultraviolet light to the perovskite solar cell can be effectively reduced, and the attenuation of the perovskite solar cell can be slowed down. By comparing Example 2 with Example 1, it can be seen that by further setting an AB glue protective layer, the damage of ultraviolet light to the perovskite solar cell can be further reduced, and the attenuation of the perovskite solar cell can be better slowed down. In this way, it is further proved that the protective layer effectively protects the ultraviolet light absorbing layer and prevents it from being damaged by water and oxygen in the external environment.

[0074] The transmittance of the four-layer stacked structure of the UV cutoff film, substrate, first electrode layer and hole transport layer in Example 1 was tested, and the transmittance of the three-layer stacked structure of the substrate, first electrode layer and hole transport layer in Comparative Example 1 was tested. The test results can be referred to Figure 6 .Depend on Figure 6 It can be seen that the transmittance of the four-layer stacked structure of the UV cutoff adhesive film, the substrate, the first electrode layer and the hole transport layer in Example 1 to ultraviolet light in the ultraviolet light band (300-400nm) is basically 0, while the transmittance to visible light is relatively high. The transmittance of the three-layer stacked structure of the substrate, the first electrode layer and the hole transport layer in Comparative Example 1 to ultraviolet light in the ultraviolet light band (300-400nm) is relatively high, basically above 48%.

[0075] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0076] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the utility model. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0077] Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in the field can change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A UV cut-off film, It is characterized in that include: An ultraviolet light absorbing layer, wherein the ultraviolet light absorbing layer comprises bis-ethylhexyloxyphenol methoxyphenyl triazine, A protective layer, wherein the protective layer is arranged on one side of the ultraviolet light absorbing layer, and a side of the protective layer away from the ultraviolet light absorbing layer is a light receiving surface, The protective layer is a transparent adhesive, and the transparent adhesive is an AB adhesive layer. The raw materials of the AB adhesive layer are composed of adhesive A and hardener B, the mixing ratio of the adhesive A and the hardener is 1:1, the adhesive A is acrylic modified epoxy resin, and the hardener B is a modified amine hardener.

2. The UV cutoff film according to claim 1, It is characterized in that The thickness of the ultraviolet light absorbing layer is 500 nanometers to 1 micrometer.

3. The UV cutoff film according to claim 1, It is characterized in that The thickness of the protective layer is 0.5 to 1 mm.

4. A solar cell, It is characterized in that include: The UV cutoff film according to any one of claims 1 to 3.

5. The solar cell according to claim 4, It is characterized in that The solar cell is a perovskite solar cell, and the perovskite solar cell comprises: A substrate having a first surface and a second surface disposed opposite to each other; A perovskite battery chip, wherein the perovskite battery chip is arranged on one side of the first surface; The ultraviolet light absorbing layer in the ultraviolet cut-off adhesive film is arranged on one side of the second surface, The protective layer in the UV cut-off adhesive film is arranged on a side of the UV light absorbing layer away from the substrate.

6. The solar cell according to claim 5, It is characterized in that The perovskite battery chip comprises: A first electrode layer, wherein the first electrode layer is arranged on a side close to the first surface; a first charge transport layer, wherein the first charge transport layer is disposed on a side of the first electrode layer away from the substrate; A perovskite light absorbing layer, wherein the perovskite light absorbing layer is disposed on a side of the first charge transport layer away from the substrate; A second charge transport layer, wherein the second charge transport layer is disposed on a side of the perovskite light absorbing layer away from the substrate; A second electrode layer is disposed on a side of the second charge transport layer away from the substrate.

Citation Information

Cited By

  • Semi-cut-off packaging material and preparation method and application thereof