A high-precision quartz substrate glue coating and its production process

By setting a double-layer coating structure on a quartz substrate and using high-temperature resistant silicone resin, the problem of inaccurate photoresist layer development was solved, achieving high-precision inverted T-shaped pattern control and strong adhesion, thus improving the reliability of metal patterns.

CN115793397BActive Publication Date: 2024-11-05ANHUI HECHEN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211509391.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-11-05
Estimated Expiration
2042-11-29

AI Technical Summary

Technical Problem

Existing technologies make it difficult to control the development process of the photoresist layer when creating metal patterns, resulting in inaccurate pattern shapes. Furthermore, the etching process can corrode other parts of the semiconductor device, making it difficult to achieve inverted T-shaped patterns.

Method used

A double-layer quartz substrate adhesive structure is adopted. The first adhesive layer contains high-temperature resistant silicone resin material, and the second adhesive layer has a larger area ratio than the first adhesive layer. The inverted T-shaped pattern is formed by pressure treatment. The high-temperature resistant silicone resin material is not easily deformed at high temperatures, which ensures that the area ratio of the second adhesive layer is increased.

Benefits of technology

It achieves high-precision inverted T-shaped pattern control, improves the accuracy and adhesion of the photoresist pattern, avoids deformation of the photoresist layer at high temperatures, and enhances the reliability of the metal pattern.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115793397B_ABST
    Figure CN115793397B_ABST
Patent Text Reader

Abstract

The present invention discloses a high-precision quartz substrate coating and its production process, and relates to the technical field of quartz basic coating. A high-precision quartz substrate coating, the coating is provided with a double-layer structure, which is respectively a first adhesive layer bonded to the outer surface of the quartz substrate material 3 and a second adhesive layer connected to the first adhesive layer, the width ratio of the second adhesive layer is greater than the width ratio of the first adhesive layer; the first adhesive layer is made of the following materials in parts by weight: 10-20 parts of high-temperature resistant silicone resin, 30-50 parts of cresol resin, 11-13 parts of photosensitizer and 65-70 parts of additives. A high-precision quartz substrate coating and its production process proposed by the present invention, the coating is provided with a double-layer structure, and a high-temperature resistant silicone resin material is added to the material for preparing the first adhesive layer, which can withstand high temperatures and impacts. When the second adhesive layer is pressurized, the first adhesive layer is not easily deformed, ensuring that only the width of the second adhesive layer is increased, thereby achieving the shape of the coating pattern to reach an inverted T-shaped pattern.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz basic glue coating, in particular to a high-precision quartz substrate glue coating and a production process thereof. Background Art

[0002] In the semiconductor manufacturing process, metal patterns are usually used to make device leads and electrodes. These metal patterns are usually formed by photolithography followed by wet or dry etching. However, some metals are difficult to etch using wet or dry etching, and the chemicals required to etch these metal patterns will have a corrosive effect on other parts of the semiconductor device. Therefore, a lift-off process is usually used to make these metal patterns.

[0003] A Chinese patent with publication number CN113075868A discloses a photoresist patterning method and a double-layer photoresist stripping method; the method comprises: sequentially forming a first photoresist layer and a second photoresist layer on a substrate; simultaneously exposing the first photoresist layer and the second photoresist layer using a mask; performing positive development on the exposed first photoresist layer and the second photoresist layer using a positive developer to form a first opening and a second opening of equal width in the first photoresist layer and the second photoresist layer respectively; performing negative development on the first photoresist layer using a negative developer to increase the width of the first opening so that the width of the first opening is greater than the width of the second opening.

[0004] Although this application solves to a certain extent the technical problem of controlling the shape of the graphic to achieve an inverted T-shaped graphic and avoiding secondary exposure of the desired pattern in the background technology, this application uses a negative developer to negatively develop the first photoresist layer, which makes it difficult to control the first photoresist layer from being completely removed, and after the outer wall of the first photoresist layer is removed, the connection between the second photoresist layer and the first photoresist layer is exposed, and a part of the second photoresist layer will also be removed, making it difficult to achieve the desired effect. Summary of the invention

[0005] The purpose of the present invention is to provide a high-precision quartz substrate coating and its production process. The coating has a double-layer structure. A high-temperature resistant silicone resin material is added to the material for preparing the first adhesive layer. The material is resistant to high temperatures and impacts. When the second adhesive layer is pressurized, the first adhesive layer is not easily deformed, ensuring that only the width of the second adhesive layer is increased, thereby achieving an inverted T-shaped shape of the coating pattern, thereby accurately controlling the width of the second adhesive layer to solve the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solution: a high-precision quartz substrate glue coating, wherein the glue coating is provided with a double-layer structure, namely a first glue layer bonded to the outer surface of the quartz substrate material 3 and a second glue layer connected to the first glue layer, wherein the width ratio of the second glue layer is greater than the width ratio of the first glue layer;

[0007] The first adhesive layer is made of the following materials in parts by weight: 10-20 parts of high temperature resistant silicone resin, 30-50 parts of phenolic resin, 11-13 parts of photosensitizer and 65-70 parts of additives.

[0008] Preferably, the first adhesive coating processing method used in the first adhesive layer is as follows:

[0009] The high temperature resistant silicone resin and cresol resin are prepared, and a photosensitive agent, an additive and a solvent are mixed into the prepared high temperature resistant silicone resin and cresol resin, and then various indicators of the glue are adjusted to meet the requirements, and finally filtered and packaged. The photosensitive agent is made of the following raw materials in parts by weight: 4-5 parts of trihydroxybenzophenone, 7-8 parts of 215 sulfonyl chloride and 10-30 parts of acetone, and the solvent is acetone.

[0010] Preferably, the preparation method of the high temperature resistant silicone resin is as follows:

[0011] γ-methacryloxypropyltrimethoxysilane, butyl benzoate and toluene were mixed evenly, reacted under 365 nm ultraviolet light for 3 h, and the solvent was removed by reduced pressure distillation to obtain polyγ-methacryloxypropyltrimethoxysilane;

[0012] Subsequently, poly-γ-methacryloxypropyltrimethoxysilane was mixed with the side methoxysiloxane, and toluene was added to the mixture for mixing assistance, and then dibutyltin dilaurate was added, and the mixture was allowed to stand and cure at room temperature for 7 days to obtain a high temperature resistant silicone resin.

[0013] Preferably, the second adhesive layer is made of the following materials in parts by weight: 50-60 parts of phenolic resin, 11-13 parts of photosensitive agent and 65-70 parts of additives. The second coating processing method used for the second adhesive layer is as follows: prepare phenolic resin, mix photosensitive agent, additive and solvent into the phenolic resin, then adjust various indicators of the glue to meet the requirements, and finally filter and package.

[0014] Another technical problem to be solved by the present invention is to provide a production process for high-precision quartz substrate glue coating, comprising the following steps:

[0015] S1 cleaning: put the quartz substrate to be processed into the cleaning agent for cleaning. After the cleaned quartz substrate is blown dry, it is dried and sent to the glue leveling place for glue leveling;

[0016] S2 pretreatment: adsorb the lower surface of the quartz substrate, add propylene glycol methyl ether acetate as a diluent on the upper surface of the quartz substrate, drive the quartz substrate to rotate, and spread the propylene glycol methyl ether acetate on the surface of the quartz substrate. The rotation time is 20-30s;

[0017] S3: the first adhesive layer material is prepared into a first coating according to a proportion, and the first coating is coated on the surface of the quartz substrate;

[0018] S4: the second adhesive layer material is prepared into a second coating according to a proportion, and the second coating is applied on the basis of the first coating;

[0019] S5 exposure and development: using a mask plate to simultaneously expose the first coating layer and the second coating layer, and using a positive developer to positively develop the exposed first coating layer and the second coating layer to form a first coating layer and a second coating layer respectively;

[0020] S6 Increase the duty ratio: Heat the quartz substrate and cover the surface of the quartz substrate with a layer of PDMS gasket. Cover the upper surface of the PDMS gasket with thin paper and a glass press, and apply pressure to the glass press. After cooling down, remove the glass press and the thin paper to complete the adhesive layer processing.

[0021] Preferably, the step of leveling the first layer of glue in step S3 specifically comprises the following steps:

[0022] S31: dripping the first glue on the center of the surface of the quartz substrate, the quartz substrate starts to rotate, accelerates to 3000r / min within 10s, keeps rotating for 40s, and then decelerates to a stop state;

[0023] S32: The coated quartz substrate is baked at 90-100° C. for 15-20 minutes to remove the solvent in the first coating, and then cooled to room temperature.

[0024] Preferably, the step of applying the second layer of adhesive in step S4 specifically comprises the following steps:

[0025] S41: On the basis of the first glue layer, a second glue coating is dripped on the center of the surface of the quartz substrate, and the quartz substrate starts to rotate, accelerates to 2000r / min within 10s, keeps rotating for 30s, and then decelerates to a stop state;

[0026] S42: The coated quartz substrate is baked at 90-100° C. for 20-30 minutes to remove the solvent in the second coating, and then cooled to room temperature.

[0027] Preferably, the step S6 of increasing the duty ratio specifically comprises the following steps:

[0028] S61: bringing the bottom surface of the quartz substrate into contact with the heating platform, covering the surface of the second adhesive layer with a layer of PDMS gasket, and heating the quartz substrate and the PDMS gasket at the same time;

[0029] S62: heating to the glass transition temperature of the second adhesive layer, laying a thin paper sheet and a glass substrate on the PDMS gasket, and applying vertical pressure to the glass substrate;

[0030] S63: After the pressure is applied, the temperature is lowered to room temperature, and the glass substrate, thin paper sheet and PDMS gasket are removed.

[0031] Preferably, the glass transition temperature of the second adhesive layer is 150°C-170°C.

[0032] Preferably, the load of vertically applying pressure to the glass substrate is 100 kPa-200 kPa, and the pressure application time is 30-50 minutes.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The coating of the present invention is provided with a double-layer structure. A high-temperature resistant silicone resin material is added to the material for preparing the first adhesive layer, which is resistant to high temperatures and impacts. When the second adhesive layer is pressurized, the first adhesive layer is not easily deformed, ensuring that only the width of the second adhesive layer is increased, thereby achieving an inverted T-shaped coating pattern;

[0035] 2. Before applying glue to the quartz substrate, the present invention drips propylene glycol methyl ether acetate as a diluent on the surface of the quartz substrate to increase the wettability of the surface of the quartz substrate, accelerate the bonding of the subsequent first layer of glue with the quartz substrate, improve the firmness of the bonding, and further prevent the first glue layer from deforming when under pressure;

[0036] 3. The thickness of the first adhesive layer in the present invention is smaller than that of the second adhesive layer, which provides a basis for changing the width of the second adhesive layer. When the pressure load is changed, the width ratio of the second adhesive layer to the first adhesive layer can be changed, thereby accurately controlling the width of the second adhesive layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] See also Figure 1 , a high-precision quartz substrate glue coating, the glue coating is provided with a double-layer structure, namely a first glue layer bonded to the outer surface of the quartz substrate material 3 and a second glue layer connected to the first glue layer, the width ratio of the second glue layer is greater than the width ratio of the first glue layer;

[0040] The first adhesive layer is made of the following materials in parts by weight: 10-20 parts of high temperature resistant silicone resin, 30-50 parts of phenolic resin, 11-13 parts of photosensitizer and 65-70 parts of additives.

[0041] The first glue coating process used in the first glue layer is as follows:

[0042] The high temperature resistant silicone resin and cresol resin are prepared, and a photosensitive agent, an additive and a solvent are mixed into the prepared high temperature resistant silicone resin and cresol resin, and then various indicators of the glue are adjusted to meet the requirements, and finally filtered and packaged. The photosensitive agent is made of the following raw materials in parts by weight: 4-5 parts of trihydroxybenzophenone, 7-8 parts of 215 sulfonyl chloride and 10-30 parts of acetone, and the solvent is acetone.

[0043] The processing process of the photosensitive agent is as follows: add trihydroxybenzophenone and 2,15 sulfonyl chloride to acetone and dissolve under stirring. After complete dissolution, add organic alkali solution as a catalyst, control the reaction temperature at 30-35°C, and after the addition is completed, continue the reaction for 1 hour. Rinse the reaction solution into water, precipitate the photosensitive agent, centrifuge and dry to obtain the photosensitive agent.

[0044] The process of synthesizing cresol-formaldehyde resin is as follows: the raw materials of mixed cresol and formaldehyde are sent into a stainless steel kettle, an appropriate amount of oxalic acid is added as a catalyst, heated to reflux reaction for 5 to 6 hours, and then water and unreacted monomer phenol are removed by reduced pressure distillation to obtain cresol-formaldehyde resin.

[0045] The preparation method of high temperature resistant silicone resin is as follows:

[0046] γ-methacryloxypropyltrimethoxysilane, butyl benzoate and toluene were mixed evenly, reacted under 365 nm ultraviolet light for 3 h, and the solvent was removed by reduced pressure distillation to obtain polyγ-methacryloxypropyltrimethoxysilane;

[0047] Subsequently, poly-γ-methacryloxypropyltrimethoxysilane was mixed with the side methoxysiloxane, and toluene was added to the mixture for mixing assistance, and then dibutyltin dilaurate was added, and the mixture was allowed to stand and cure at room temperature for 7 days to obtain a high temperature resistant silicone resin.

[0048] The second adhesive layer is made of the following materials in parts by weight: 50-60 parts of phenolic resin, 11-13 parts of photosensitive agent and 65-70 parts of additives. The second coating processing method used for the second adhesive layer is as follows: prepare phenolic resin, mix photosensitive agent, additive and solvent into phenolic resin, then adjust various indicators of the glue to meet the requirements, and finally filter and package.

[0049] In order to better demonstrate the production process of high-precision quartz substrate gluing, this embodiment now proposes a production process of high-precision quartz substrate gluing, including the following steps:

[0050] S1 cleaning: put the quartz substrate to be processed into the cleaning agent for cleaning. After the cleaned quartz substrate is blown dry, it is dried and sent to the glue leveling place for glue leveling;

[0051] S2 pretreatment: adsorb the lower surface of the quartz substrate, add propylene glycol methyl ether acetate as a diluent on the upper surface of the quartz substrate, drive the quartz substrate to rotate, and spread the propylene glycol methyl ether acetate on the surface of the quartz substrate. The rotation time is 20-30s. Through pretreatment, the wettability of the surface of the quartz substrate is increased, the subsequent first layer of glue is bonded to the quartz substrate, and the firmness of the bonding is improved;

[0052] S3: the first adhesive layer material is prepared into a first coating according to a proportion, and the first coating is coated on the surface of the quartz substrate;

[0053] The specific steps include:

[0054] S31: dripping the first glue on the center of the surface of the quartz substrate, the quartz substrate starts to rotate, accelerates to 3000r / min within 10s, keeps rotating for 40s, and then decelerates to a stop state. Under high-speed rotation, the first glue is evenly connected to the surface of the quartz substrate;

[0055] S32: The coated quartz substrate is baked at 90-100° C. for 15-20 minutes to remove the solvent in the first coating, and then dried to room temperature. After drying, the thickness of the first layer of glue is 1-2 um.

[0056] S4: the second adhesive layer material is prepared into a second coating according to a proportion, and the second coating is applied on the basis of the first coating;

[0057] The specific steps include:

[0058] S41: On the basis of the first glue layer, a second glue coating is dripped on the center of the surface of the quartz substrate, and the quartz substrate starts to rotate, accelerates to 2000r / min within 10s, keeps rotating for 30s, and then decelerates to a stop state. The rotation speed is lower when the second glue layer is applied, so that the coating thickness of the second glue layer is thicker;

[0059] S42: The coated quartz substrate is baked at 90-100° C. for 20-30 minutes to remove the solvent in the second coating, and then cooled to room temperature. The thickness of the second layer of glue is 2-3 um.

[0060] S5 exposure and development: using a mask plate to simultaneously expose the first and second adhesive layers, and using a positive developer to positively develop the exposed first and second adhesive layers to form a first adhesive layer and a second adhesive layer, respectively. At this time, the widths of the first and second adhesive layers are the same;

[0061] S6: Increase the duty ratio: Heat the quartz substrate, and cover the surface of the quartz substrate with a layer of PDMS gasket, cover the upper surface of the PDMS gasket with thin paper and glass pressing sheet, and apply pressure to the glass pressing sheet. After cooling down, remove the glass pressing sheet and thin paper to complete the adhesive layer processing;

[0062] The specific steps include:

[0063] S61: bringing the bottom surface of the quartz substrate into contact with the heating platform, covering the surface of the second adhesive layer with a layer of PDMS gasket, and heating the quartz substrate and the PDMS gasket at the same time;

[0064] S62: heating to the glass transition temperature of the second adhesive layer, the glass transition temperature of the second adhesive layer is 150°C-170°C, laying a thin paper sheet and a glass substrate on the PDMS gasket, applying vertical pressure to the glass substrate, the load of the vertical pressure on the glass substrate is 100kPa-200kPa, and the pressure time is 30-50 minutes. At high temperature, the second adhesive layer is converted into a plastic state, and the width ratio of the second adhesive layer is increased by applying pressure through the glass substrate. The width of the second adhesive layer is greater than the width of the first adhesive layer, and the shape of the pattern reaches an inverted T-shaped pattern;

[0065] S63: After the pressure is applied, the temperature is lowered to room temperature, and the glass substrate, thin paper sheet and PDMS gasket are removed.

[0066] Different weight portions of materials were taken to prepare the first coating and the second coating, and different ratios of the first coating and the second coating were used to prepare the coating of the quartz substrate, and the coating data in Examples 1 to 3, Comparative Examples 1 and 2 were obtained, wherein the high temperature resistant silicone resin material was missing in Comparative Example 1, and the quartz substrate was not pretreated in Comparative Example 2, as follows:

[0067]

[0068] It can be concluded from the above table that in Examples 1 to 3, the width of the second adhesive layer is different from that of the first adhesive layer, and the width of the second adhesive layer is greater than that of the first adhesive layer, which can achieve an inverted T-shaped pattern, and is convenient for metal stripping. In Example 2, the specific gravity of the high-temperature resistant silicone resin is the highest, and the deformation of the first adhesive layer after processing is the smallest, so that the width ratio of the second adhesive layer to the first adhesive layer is the largest. In Comparative Example 1, because the high-temperature resistant silicone resin is not used, the second adhesive layer and the first adhesive layer are deformed under load, and the width ratio does not change. In Comparative Example 2, because the quartz substrate is not pre-treated, the bonding firmness between the quartz substrate and the first adhesive layer is not enough, and the first adhesive layer also undergoes a certain deformation, and the width ratio of the second adhesive layer to the first adhesive layer does not change much. At the same time, when the pressure increases, the width ratio of the second adhesive layer to the first adhesive layer increases accordingly, and the temperature has little effect on the width ratio.

[0069] In summary, the present invention proposes a high-precision quartz substrate coating and its production process, the coating has a double-layer structure, and a high-temperature resistant silicone resin material is added to the material for preparing the first adhesive layer, which can withstand high temperatures and impacts. When the second adhesive layer is pressurized, the first adhesive layer is not easy to deform, ensuring that only the width of the second adhesive layer is increased, thereby achieving an inverted T-shaped pattern of the coating pattern; before the quartz substrate is coated with glue, propylene glycol methyl ether acetate is dripped on the surface of the quartz substrate as a diluent to increase the wettability of the surface of the quartz substrate, accelerate the subsequent bonding of the first layer of glue to the quartz substrate, improve the firmness of the bonding, and further prevent the first adhesive layer from deforming when under pressure; the uniform glue thickness during processing of the first adhesive layer is less than the uniform glue thickness of the second adhesive layer, providing a basis for changing the width of the second adhesive layer, and when the pressurized load is changed, the width ratio of the second adhesive layer to the first adhesive layer can be changed, thereby accurately controlling the width of the second adhesive layer.

[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A production process for high-precision quartz substrate gluing, characterized in that: The produced adhesive coating is provided with a double-layer structure, which comprises a first adhesive layer bonded to the outer surface of the quartz substrate material and a second adhesive layer connected to the first adhesive layer, wherein the width ratio of the second adhesive layer is greater than the width ratio of the first adhesive layer; The first adhesive layer is made of the following materials in parts by weight: 10-20 parts of high temperature resistant silicone resin, 30-50 parts of cresol resin, 11-13 parts of photosensitizer and 65-70 parts of additives; The second adhesive layer is made of the following materials in parts by weight: 50-60 parts of cresol resin, 11-13 parts of photosensitizer and 65-70 parts of additives. The second adhesive layer is processed by the following second coating method: preparing cresol resin, mixing photosensitizer, additive and solvent into cresol resin, and finally filtering and packaging; The production process of high-precision quartz substrate glue coating includes the following steps: S1 cleaning: put the quartz substrate to be processed into the cleaning agent for cleaning. After the cleaned quartz substrate is blown dry, it is dried and sent to the glue leveling place for glue leveling; S2 pretreatment: adsorb the lower surface of the quartz substrate, add propylene glycol methyl ether acetate as a diluent on the upper surface of the quartz substrate, drive the quartz substrate to rotate, and spread the propylene glycol methyl ether acetate on the surface of the quartz substrate. The rotation time is 20-30s; S3: the first adhesive layer material is prepared into a first coating according to a proportion, and the first coating is coated on the surface of the quartz substrate; S4: the second adhesive layer material is prepared into a second coating according to a proportion, and the second coating is applied on the basis of the first coating; S5 exposure and development: using a mask plate to simultaneously expose the first coating layer and the second coating layer, and using a positive developer to positively develop the exposed first coating layer and the second coating layer to form a first coating layer and a second coating layer respectively; S6 Increase the duty ratio: Heat the quartz substrate and cover the surface of the quartz substrate with a layer of PDMS gasket. Cover the upper surface of the PDMS gasket with thin paper and a glass press, and apply pressure to the glass press. After cooling down, remove the glass press and the thin paper to complete the adhesive layer processing.

2. The production process for high-precision quartz substrate glue coating as claimed in claim 1, characterized in that: The first glue coating processing method used in the first glue layer is as follows: The high temperature resistant silicone resin and cresol formaldehyde resin are prepared, and a photosensitive agent, an additive and a solvent are mixed into the prepared high temperature resistant silicone resin and cresol formaldehyde resin, and finally filtered and packaged. The photosensitive agent is prepared from the following raw materials in parts by weight: 4-5 parts of trihydroxybenzophenone, 7-8 parts of 215 sulfonyl chloride and 10-30 parts of acetone, and the solvent is acetone.

3. The production process for high-precision quartz substrate glue coating as claimed in claim 2, characterized in that: The preparation method of the high temperature resistant silicone resin is as follows: γ-methacryloxypropyltrimethoxysilane, butyl benzoate and toluene were mixed evenly, reacted under 365 nm ultraviolet light for 3 h, and the solvent was removed by reduced pressure distillation to obtain polyγ-methacryloxypropyltrimethoxysilane; Subsequently, poly-γ-methacryloxypropyltrimethoxysilane was mixed with the side methoxysiloxane, and toluene was added to the mixture for mixing assistance, and then dibutyltin dilaurate was added, and the mixture was allowed to stand and cure at room temperature for 7 days to obtain a high temperature resistant silicone resin.

4. The production process for high-precision quartz substrate glue coating as claimed in claim 1, characterized in that: The step S3 of evenly distributing the first layer of glue specifically comprises the following steps: S31: dripping the first glue on the center of the surface of the quartz substrate, the quartz substrate starts to rotate, accelerates to 3000r / min within 10s, keeps rotating for 40s, and then decelerates to a stop state; S32: The coated quartz substrate is baked at 90-100° C. for 15-20 minutes to remove the solvent in the first coating, and then cooled to room temperature.

5. The production process for high-precision quartz substrate glue coating as claimed in claim 1, characterized in that: The step of applying the second layer of glue in step S4 specifically comprises the following steps: S41: On the basis of the first glue layer, a second glue coating is dripped on the center of the surface of the quartz substrate, and the quartz substrate starts to rotate, accelerates to 2000r / min within 10s, keeps rotating for 30s, and then decelerates to a stop state; S42: The coated quartz substrate is baked at 90-100° C. for 20-30 minutes to remove the solvent in the second coating, and then cooled to room temperature.

6. The production process for high-precision quartz substrate glue coating as claimed in claim 1, characterized in that: The step of increasing the duty ratio in step S6 specifically includes the following steps: S61: bringing the bottom surface of the quartz substrate into contact with the heating platform, covering the surface of the second adhesive layer with a layer of PDMS gasket, and heating the quartz substrate and the PDMS gasket at the same time; S62: heating to the glass transition temperature of the second adhesive layer, laying a thin paper sheet and a glass substrate on the PDMS gasket, and applying vertical pressure to the glass substrate; S63: After the pressure is applied, the temperature is lowered to room temperature, and the glass substrate, thin paper sheet and PDMS gasket are removed.

7. The production process for high-precision quartz substrate glue coating as claimed in claim 6, characterized in that: The glass transition temperature of the second adhesive layer is 150°C-170°C.

8. The production process for high-precision quartz substrate glue coating as claimed in claim 6, characterized in that: The load of vertically applying pressure to the glass substrate is 100 kPa-200 kPa, and the pressure application time is 30-50 minutes.