A porous ceramic material with cross-scale Haversian tube-like structure and its preparation method and metal mold
Through the porous ceramic material with a cross-scale imitation of Haval tube structure, combined with the multi-stage porous structure design of organic material carriers and ceramics, the problems of mismatch in mechanical properties and poor biocompatibility of existing bone defect repair materials are solved, and the lightness of ceramic materials is achieved Quality, high strength and biocompatible, suitable for bone repair and multi-field applications.
Patent Information
- Application Number
- CN202310525624.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-10
AI Technical Summary
The mechanical properties of existing bone defect repair materials do not match the natural bone, resulting in stress shielding and loose implants, and there is a risk of pathogenicity related to autologous bone donors and high cost and poor biological activity of metal materials, making it difficult to achieve multifunctionality. Porous structure design.
Porous ceramic materials with a cross-scale imitation of Haval tube structure are used to form a multi-stage porous structure through the combination of organic support and ceramics, including large-scale through-holes and small-scale micropores. The ceramics are grown on the organic support in situ to form excellent Mechanical properties and biocompatibility.
Ceramic materials with multi-scale pore structures are lightweight and high-strength, suitable for bone repair and other fields, and have good biocompatibility, which can induce vascularization and cell migration, and are suitable for bone repair and other applications. .
Smart Images

Figure CN116553907B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of porous ceramic materials, and more specifically to a porous ceramic material with a cross-scale Haversian tube-like structure and a preparation method and a metal mold thereof. Background Art
[0002] Although bone tissue has a natural regenerative capacity sufficient to repair small damaged sites, such as cracks and certain types of fractures, bone defects that are usually larger than a critical size threshold of two centimeters are difficult to heal naturally and require clinical intervention. Currently, bone fixation using autologous bone, allogeneic bone, or bioinert metal devices is the current gold standard treatment for large bone defects. However, the use of autologous bone often leads to additional morbidity related to donor site healing; the use of allogeneic bone is associated with the risk of disease transmission from the donor material, and metal materials have poor bioactivity and high prices, and usually require secondary surgery for resection. At the same time, due to their incompatibility with natural bone in mechanical properties, they are prone to stress shielding, thereby causing absorption of adjacent bone tissue, and ultimately leading to loosening and failure of the implant; the field of bone tissue engineering has witnessed substantial development towards materials that induce bone regeneration processes at defect sites without incurring these risks.
[0003] With the rapid development of tissue engineering technology, a series of biomaterials have been designed into porous scaffolds for bone defect repair, because porous scaffolds can provide three-dimensional space for the implantation of blood vessels and new bone tissue. The ideal bone repair scaffold should have superior structural characteristics to provide an osteogenesis microenvironment while eliminating the interference of fibrous tissue on normal bone regeneration. Some previous studies have shown that compared with scaffolds with random porous structures, scaffolds with oriented porous structures are more conducive to cell infiltration and migration, exchange of nutrients and waste, and deposition of extracellular matrix. It should be emphasized that the above-mentioned bone scaffold functions are realized by pore structures with different pore sizes. Large pores are conducive to material transport, while micropores are conducive to cell attachment and migration. Although a variety of bone scaffolds with oriented porous structures have been effectively designed through 3D printing or oriented freeze casting technology, their pore sizes are single and it is difficult to achieve the combination of multiple functions. Therefore, how to construct a ceramic-based material with a multi-level sub-porous structure is a current difficulty. This ceramic-based material with a multi-level sub-porous structure can not only be used in the field of bone repair, but also has the potential to be used in the aerospace and military fields. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a cross-scale porous ceramic material with a Haversian tube-like structure, a preparation method thereof, and a metal mold. The cross-scale porous ceramic material with a Haversian tube-like structure has a multi-scale anisotropic pore structure, the pore structure of which is controllable, and has excellent mechanical properties; the preparation method of the cross-scale porous ceramic material with a Haversian tube-like structure is scalable.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A porous ceramic material with a cross-scale Haversian tube-like structure, comprising a plurality of Haversian tube-like structural units; the Haversian tube-like structural units are composed of an organic carrier and a ceramic loaded on the organic carrier;
[0007] The organic carrier has a multi-level pore structure;
[0008] The multi-level holes include through holes and micro holes;
[0009] The through holes and micro holes are in different directions;
[0010] The through hole has a larger pore diameter than the micropore;
[0011] The mass ratio of the organic carrier to the ceramic is 1:(0.1-2).
[0012] In the present invention, the multi-level pores include large-scale through holes and small-scale layered micropores; the ceramic is preferably grown on an organic carrier in a deposition manner. During the in-situ growth process, due to the strong interaction between the inorganic and organic carriers, the ceramic is not simply deposited on the surface of the organic matter, but through intermolecular forces, the two are fused with each other to form an integrated structure.
[0013] In the present invention, the micropores are distributed around the through holes; the through holes and the micropores are interconnected;
[0014] The micropore has a small aperture on the side close to the through hole, and a large aperture on the side away from the through hole; as the distance between the micropore and the through hole increases, the aperture of the micropore gradually increases;
[0015] The aperture of the through hole is ≥400 μm, preferably 0.4-2 mm, and the length of the through hole is >100 μm, preferably 1-15 mm;
[0016] The average pore size of the micropores is ≤100 μm, preferably 1 to 20 μm, and the length of the micropores is >10 μm, preferably 0.5 to 5 mm.
[0017] In the present invention, the number of the Haversian tube-like structural units is 1 to 50.
[0018] In the present invention, the mass ratio of the organic carrier to the ceramic is preferably 1:(0.25-1.5); in one embodiment of the present invention, the mass ratio of the organic carrier to the ceramic is 1:1.
[0019] In one embodiment of the present invention, the porous ceramic material with a cross-scale Haversian tube-like structure contains 25 Haversian tube-like structure units, the through holes of the Haversian tube-like structure units are parallelly distributed, the length of the through holes is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length is 2 mm. In the porous ceramic material with a cross-scale Haversian tube-like structure of the present invention, the micropores and the through holes are interconnected, and the overall structure is similar to the Haversian tube structure in dense bone.
[0020] When bioceramic materials are used, the cross-scale Haversian tube-like porous ceramic material of the present invention has good biocompatibility and can be used in the field of bone repair, wherein the through holes have the ability to induce vascularization and osteogenesis, and are beneficial to the deposition of mineralized extracellular matrix and vascular infiltration, while the micropores are beneficial to cell attachment and the interconnectivity between the through holes is beneficial to cell migration and material transfer.
[0021] In the present invention, the organic carrier includes one or more of a silk protein framework, a sodium alginate framework, a polyvinyl alcohol framework, a collagen framework, a chitin framework, a gelatin framework, and a sodium polystyrene sulfonate framework.
[0022] In the present invention, the ceramic is one or more of calcium carbonate, barium carbonate, hydroxyapatite, silicon dioxide, iron oxide, aluminum oxide, titanium oxide, zirconium oxide, silicon oxide, silicon carbide, and boron nitride;
[0023] The particle size of the ceramic is 10-200 nm.
[0024] The present invention also provides a metal mold, comprising a housing cavity for carrying a coolant and a molding column group arranged at the outer bottom of the housing cavity; the number, diameter and gaps between the molding columns can be adjusted according to specific needs;
[0025] The forming column group includes a plurality of forming columns.
[0026] In the present invention, the forming column group includes forming columns distributed in an array;
[0027] The gap between adjacent molding columns is >10 μm, preferably 2 mm;
[0028] The length of the molded column is >100 μm and the diameter is >400 μm.
[0029] In the present invention, the number of the forming columns is 2 to 50, preferably 25 to 50;
[0030] The gap between adjacent molding columns is >10 μm, preferably 2 mm;
[0031] The length of the molded column is >100 μm, preferably 1 to 15 mm, and the diameter of the molded column is >400 μm, preferably 0.4 to 2 mm.
[0032] In the present invention, the accommodating cavity and the forming column group form an integral structure; the forming column is preferably a cylinder;
[0033] The material of the metal mold is preferably one or more of aluminum, copper, and silver, preferably copper.
[0034] In one embodiment of the present invention, the metal mold consists of a accommodating cavity and a molding column, and the accommodating cavity and the molding column group form an integrated structure; the molding column group is a 5*5 array of metal copper cylinders with a diameter of 1mm and a gap of 2mm between columns.
[0035] The present invention also provides a method for preparing the above-mentioned porous ceramic material with a cross-scale Haversian tube-like structure, comprising:
[0036] a. contacting the organic solution with the metal mold, freezing the metal mold, and removing the metal mold to obtain an organic carrier;
[0037] b. mixing the organic carrier obtained in step a with the ceramic precursor mother solution to obtain a porous ceramic material with a cross-scale Haversian tube-like structure;
[0038] The organic solution includes one or more of a silk protein solution, a sodium alginate solution, a polyvinyl alcohol solution, a collagen solution, a chitin solution, a gelatin solution, and a sodium polystyrene sulfonate solution.
[0039] In the present invention, the metal mold includes a receiving cavity for carrying a coolant and a forming column group arranged at the outer bottom of the receiving cavity; the number, diameter and gap between the forming columns can be adjusted according to specific needs;
[0040] The forming column group includes a plurality of forming columns.
[0041] In the present invention, the forming column group includes forming columns distributed in an array;
[0042] The gap between adjacent molding columns is >10 μm, preferably 2 mm;
[0043] The length of the molded column is >100 μm and the diameter is >400 μm.
[0044] In the present invention, the number of the forming columns is 2 to 50;
[0045] The gap between adjacent molding columns is >10 μm, preferably 2 mm;
[0046] The length of the molded column is >100 μm, preferably 1 to 15 mm, and the diameter of the molded column is >400 μm, preferably 0.4 to 2 mm.
[0047] In the present invention, the accommodating cavity and the forming column group form an integral structure; the forming column is preferably a cylinder;
[0048] The material of the metal mold is preferably one or more of aluminum, copper, and silver, preferably copper.
[0049] In one embodiment of the present invention, the metal mold consists of a accommodating cavity and a molding column, and the accommodating cavity and the molding column group form an integrated structure; the molding column group is a 5*5 array of metal copper cylinders with a diameter of 1mm and a gap of 2mm between columns.
[0050] In the present invention, it is preferred that before the organic solution is brought into contact with the metal mold, 1 to 5 copper pillars with a diameter of 0.3 to 0.5 mm are inserted between the arrays of the metal mold.
[0051] In the present invention, the concentration of the organic solution is 1-4w / v%, preferably 1-2w / v%;
[0052] The organic carrier obtained in step a of the present invention has a multi-level pore structure imitating a Haversian tube.
[0053] In the present invention, the method for preparing the organic solution comprises:
[0054] Mixing the organic matter with the solvent and adjusting the pH to obtain an organic solution; the solvent is preferably water; and the mixing time is 12-16 hours;
[0055] The method for preparing the organic solution preferably comprises:
[0056] Mix water and organic matter, stir, add acetic acid, stir, and finally obtain an organic solution; the ratio of the organic matter to the solvent is 1:(40-50) g / ml; the stirring speed is 300-500 rpm; preferably, acetic acid is used to adjust the pH.
[0057] In the present invention, it is preferred to insert the metal mold into the organic solution;
[0058] The freezing of the metal mold is achieved by injecting a refrigerant into the metal mold;
[0059] The freezing also includes freezing at a pressure of 4-10 mbar, -80°C, and for 70-72 hours;
[0060] The refrigerant is one or more of liquid nitrogen, dry ice or pre-cooled ethanol solution.
[0061] In the present invention, the method of step a specifically comprises:
[0062] The organic solution is placed in a container, and a metal mold is inserted into the solution, and metal pillars are randomly inserted between the arrays. A refrigerant is then introduced into the upper part of the metal mold to freeze the organic solution, and then placed in a freeze dryer for 70-72 hours at a pressure of 4-10 mbar and a cold trap temperature of -80°C. The metal mold is removed to obtain a primary organic carrier, and the organic carrier is immersed in a mixed solution of methanol and acetic anhydride with a volume ratio of 9:1 for acetylation reaction, and then washed with water to obtain an organic carrier.
[0063] In the present invention, the concentration of the ceramic precursor in the ceramic precursor mother solution is 1-4wt%; in an embodiment of the present invention, the concentration of the ceramic precursor is 10-15mM;
[0064] The ceramic precursor is one or more of a calcium carbonate precursor, a barium carbonate precursor, a hydroxyapatite precursor, a silicon dioxide precursor, an iron oxide precursor, an aluminum oxide precursor, a titanium oxide precursor, a zirconium oxide precursor, a silicon oxide precursor, a silicon carbide precursor, a boron nitride precursor, tetrabutyl titanate, and tetraethyl silicate, preferably one or more of a calcium carbonate precursor, a barium carbonate precursor, a hydroxyapatite precursor, tetrabutyl titanate, and tetraethyl silicate;
[0065] The particle size of the ceramic precursor is 5-25nm; the ceramic precursor of the present invention is deposited in an organic carrier by in-situ growth. Compared with simple mixing, the advantages of in-situ growth are as follows: the organic and inorganic substances are more firmly combined and the interaction is stronger; in-situ growth can control the micro-nano structure of inorganic substances through thermodynamic or kinetic factors such as polyelectrolytes, temperature, pH, etc., thereby controlling their mechanical properties.
[0066] The ceramic precursor mother solution also includes a polyelectrolyte;
[0067] The concentration of the polyelectrolyte is 6-50 mM;
[0068] The polyelectrolyte is an anionic polymer and / or a cationic polymer;
[0069] The anionic polymer is polyacrylic acid;
[0070] The cationic polymer is polyacrylamine salt. A proper amount of polyelectrolyte can regulate the growth of ceramics.
[0071] In the present invention, the method for preparing the ceramic precursor mother solution comprises:
[0072] mixing a ceramic precursor with a solvent and a polyelectrolyte to obtain a ceramic precursor mother solution;
[0073] The mixing temperature is 20-30°C and the mixing time is 1-2h;
[0074] The solvent is preferably water;
[0075] The volume ratio of the polyelectrolyte to the solvent is 1:(100-1000);
[0076] In one embodiment of the present invention, the method for preparing the ceramic precursor mother solution comprises:
[0077] The tetrabutyl titanate solution, ceramic growth regulator and water were mixed, the pH of the solution was adjusted to 7-8, and polyacrylic acid (molecular weight 1800, final concentration 0.6 mM) was added;
[0078] The ceramic growth regulator is preferably magnesium chloride.
[0079] In one embodiment of the present invention, the method for preparing the ceramic precursor mother solution comprises:
[0080] Calcium carbonate powder was added to 1L of water and stirred in a constant temperature water tank at 25°C for 1 hour, during which carbon dioxide was continuously introduced; after the reaction was completed, the solution was filtered to remove solid calcium carbonate and retain the supernatant, with a final calcium ion concentration of 10mM; 400mL of the above supernatant was taken, and 4.8mL of 2mM magnesium chloride hexahydrate and 1.2mL of 0.2mM polyacrylic acid with a molecular weight of 1800 were added thereto.
[0081] In the present invention, the temperature for mixing the organic carrier and the ceramic precursor mother solution is 40-50° C. and the time is more than 12 days.
[0082] In the present invention, the step b preferably comprises:
[0083] At 40°C, the ceramic precursor mother liquor is poured into the organic carrier for at least 12 days. The ceramic precursor mother liquor is replaced on the fourth and seventh days, respectively. The optimal ceramic precursor mother liquor flow rates for 1-4 days, 4-7 days, and 7-12 days are 25 mL / min, 50 mL / min, and 15 mL / min, respectively. After the frame is converted into a ceramic frame, it is taken out and washed with ultrapure water, and then the water is replaced with an organic solvent, and then supercritically dried to obtain a Haversian tube-like ceramic-based material.
[0084] The beneficial effects of the present invention are embodied in:
[0085] 1. The present invention combines modeled freeze-drying technology and in-situ growth to prepare a cross-scale Haversian tube-like porous ceramic material with a multi-scale anisotropic pore structure. The cross-scale Haversian tube-like porous ceramic material of the present invention has multi-scale pores, including through holes greater than 400 μm that penetrate the material, and layered micropores less than 100 μm surrounding the through holes, and the micropores and through holes are interconnected, and the overall structure is similar to the Haversian tube structure in dense bone. In addition, the cross-scale Haversian tube-like porous ceramic material has excellent properties such as light weight and high strength.
[0086] 2. The method provided by the present invention is simple and reliable, the raw materials are easily available, the price is low, and the time consumption is short. It is suitable for large-scale industrial promotion and application, and provides a new means for preparing lightweight and high-strength biomimetic structural ceramic materials. The prepared materials can be used in the fields of biomedicine, aerospace, military protection, etc. When bioceramics are used, the porous ceramic material with a cross-scale Haversian tube-like structure will have good biocompatibility and can be used in the field of bone repair, wherein the through-holes have the ability to induce vascularization and osteogenesis, and are also conducive to the deposition of mineralized extracellular matrix and vascular infiltration, while the micropores are conducive to cell attachment and the interconnectivity between the through-holes is conducive to cell migration and material transport. BRIEF DESCRIPTION OF THE DRAWINGS
[0087] Figure 1 This is a structural diagram of the copper mold used in Example 1 of the present invention;
[0088] Figure 2 This is a physical picture of the copper mold used in Example 1 of the present invention;
[0089] Figure 3 This is a physical picture of the chitosan framework in Example 1 of the present invention;
[0090] Figure 4 This is a scanned image of the chitosan framework in Example 1 of the present invention;
[0091] Figure 5 This is a scanned image of the ceramic-based material of the Haversian tube structure in Example 1 of the present invention;
[0092] Figure 6 This is a scanned image of the hydroxyapatite-chitin-Haver tube-like structure ceramic-based material of Example 2 of the present invention;
[0093] Figure 7 Verification of CCK8 cell proliferation of the Haversian tube-like ceramic-based material obtained in Example 2 of the present invention;
[0094] Figure 8 The alkaline phosphatase (ALP) staining experimental data of the Haversian tube-like ceramic-based material obtained in Example 2 of the present invention;
[0095] Fig. 9 This is a picture of a rat bone defect model manufactured using the Haversian tube-like ceramic-based material obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0096] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0097] In order to further illustrate the present invention, the following examples are provided for detailed description. The raw materials used in the following examples of the present invention are all commercially available commodities.
[0098] Example 1
[0099] This embodiment provides a calcium carbonate-chitin-haverd tube-like structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0100] 1) Preparation of chitosan solution: Weigh 2 g of chitosan powder (Chinese medicine 69047438, molecular weight about 4800 g / mol) into a 200 mL beaker, add 98 mL of deionized water, slowly drop 2 mL of acetic acid into the mixture under vigorous stirring (300 rpm), stir for 12 hours, and finally obtain a uniform 2 w / v% (20 mg / mL) chitosan solution.
[0101] 2) Measure 15 mL of the chitosan solution into a polydimethylsiloxane square mold (length 12 mm, width 12 mm, height 15 mm), and place a copper mold (such as Figure 1 , Figure 2 As shown, Figure 1 The copper mold structure diagram used in this example is Figure 2 The copper mold is inserted into the solution, and 5 copper pillars with a diameter of 0.5 mm are inserted between the arrays. Liquid nitrogen is then introduced into the upper part of the copper mold to freeze the chitosan solution, and then placed in a freeze dryer for 72 hours at a pressure of 4-10 mbar and a cold trap temperature of -80°C to obtain a chitosan framework. The chitosan framework is immersed in a mixed solution of methanol (Chinese medicine) and acetic anhydride (Chinese medicine) in a volume ratio of 9:1 for acetylation reaction. The reaction needs to be sealed and placed at 45°C for 4 hours. After the reaction, a chitin framework is obtained, such as Figure 3 As shown, wash it with ultrapure water 10 times and place it in a clean beaker filled with ultrapure water for later use.
[0102] 3) Preparation of ceramic precursor mother solution: Add excess calcium carbonate powder (Chinese medicine) to 1L ultrapure water, stir in a constant temperature water tank at 25°C for 1 hour, and continuously introduce carbon dioxide during the reaction; after the reaction is completed, filter the solution to remove the suspended calcium carbonate, and retain the supernatant, with a final calcium ion concentration of 10mM. Take 400mL of the above supernatant, add 4.8mL of 2mM magnesium chloride hexahydrate (Chinese medicine) and 1.2mL of 0.2mM polyacrylic acid with a molecular weight of 1800 (Sigma).
[0103] 4) Preparation of calcium carbonate-chitosan-Haver tube structure ceramic-based material: Cut the chitin framework obtained in the above step 2) into blocks, put them into a square silicone mold, open holes (diameter 12 mm) at both ends of the mold, and seal the mold with a clamp, place it in a 40°C oven, use a 100mL syringe (inner diameter 30mm), and use a circulating injection pump to repeatedly inject the above ceramic precursor mother liquid into the organic framework. Replace the ceramic precursor mother liquid on the fourth and seventh days, respectively. The optimal ceramic precursor mother liquid flow rates for 1-4 days, 4-7 days, and 7-12 days are 25mL / min, 50mL / min, and 15mL / min, respectively. After the frame is converted into a mineral ceramic frame, it is taken out and washed with ultrapure water three times to remove free ions, and then the water is replaced with acetone, and then supercritical drying is performed to obtain a Haversian tube structure ceramic-based material, in which the mass ratio of the chitin frame and calcium carbonate is 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0104] Figure 4 This is a scan of the chitosan framework. Figure 4 As can be seen in the figure, the through holes of the chitosan framework and the micropores distributed around the through holes. Figure 5 This is a scan of the ceramic-based material that imitates the Haversian tube structure. Figure 5 It can be seen that the microporous surface of the chitosan framework still retains a porous structure after the growth of ceramics, and the micropore size distribution is 1 to 20 μm.
[0105] Example 2
[0106] This embodiment provides a hydroxyapatite-chitin-haverd tube-like structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0107] 1) The preparation of chitosan solution is the same as that in Example 1.
[0108] The chitin framework preparation was the same as in Example 1.
[0109] 2) Preparation of ceramic precursor mother liquor: According to the 5-fold SBF scheme, 450 mL of deionized water was measured and placed in a 1 L plastic container, sodium chloride, sodium bicarbonate, sodium hydrogen phosphate dodecahydrate, and magnesium chloride hexahydrate were added in sequence to dissolve, and then polyacrylamine hydrochloride PAH (finally 20 mM) was added, and 10 mL of 1 M hydrochloric acid was added. After stirring evenly, 6.25 mL of 1 M calcium chloride solution was added dropwise, and the pH was adjusted to 6.2 with tris buffer with a pH of 9.0. Finally, the solution was fixed to 500 mL, so that the final sodium ion concentration was 733 mM, the magnesium ion concentration was 30 mM, the calcium ion concentration was 12.5 mM, the chloride ion concentration was 720 mM, the hydrogen phosphate ion concentration was 5.0 mM, and the bicarbonate ion concentration was 21 mM.
[0110] 3) The preparation of hydroxyapatite-chitin-mimic Haversian tube structure ceramic-based material is the same as that in Example 1. In this material, the mass ratio of chitin framework to hydroxyapatite is 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0111] Figure 6 This is a scan of the hydroxyapatite-chitin-Haver tube structure ceramic matrix material. Figure 6 It can be seen that the micropores of the hydroxyapatite-chitin-mimicking Haversian tube structure ceramic matrix material are covered with ceramic particles.
[0112] Taking this material as an example, biocompatibility verification was carried out using 3T3 cells to verify cytotoxicity, cell proliferation, cell differentiation, and in vivo induction of bone regeneration.
[0113] The CCK8 cell proliferation assay process is as follows:
[0114] 1) Cells were plated at a density of 2×10 4 Each well was inoculated on the sample surface of a 24-well plate.
[0115] 2) Discard the original culture medium and wash with PBS three times.
[0116] 3) Prepare CCK-8 solution at a ratio of 1:10 and operate in a dark environment.
[0117] 4) CCK-8 solution was added after 1, 4, and 7 days of culture.
[0118] 5) Incubate at 37°C for 2 hours.
[0119] 6) Take 100 μL of the solution into a 96-well plate and use an ELISA reader to measure the OD value at a wavelength of 450 nm.
[0120] 7) Statistical data was collected and graphed using Origin 2020.
[0121] The experimental results of CCK8 cell proliferation are as follows Figure 7 As shown, from Figure 7 It can be seen that the Haversian tube-like ceramic-based material of this embodiment has low cytotoxicity and has certain biocompatibility.
[0122] The alkaline phosphatase (ALP) staining experimental process is as follows:
[0123] 1) Prepare 0.02 ng / mL phenol standard solution;
[0124] 2) Add the following reagents to a 96-well plate: 50 Ul of buffer solution; 50 Ul of base solution;
[0125] 3) Incubate at 37°C in a shaker in the dark for 15 minutes;
[0126] 4) Add 150 μL of colorimetric reagent to each well
[0127] 5) Take photos
[0128] The staining results are as follows Figure 8 As shown, from Figure 8 It can be seen that the staining results of the Haversian tube-like structure material are better than those of the disordered group, indicating that the cross-scale pore structure is conducive to cell proliferation.
[0129] Fig. 9 To create a rat bone defect model, Fig. 9 The whole experimental modeling process is demonstrated. The sample size used in this experiment is 3μm in diameter and 6μm in height (cylinder).
[0130] Example 3
[0131] This embodiment provides a hydroxyapatite-silk protein-haverd tube-like structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0132] 1) Silk protein extraction: The first step is degumming. The dried cocoons are cut into small pieces and placed in a 2L hot sodium carbonate solution with a concentration of 0.02 mol / L. The cocoons are stirred magnetically for 30 minutes until they gradually dissolve and disappear into white filaments. They are rinsed with deionized water 3-5 times and dried in a 35°C oven for 2 days. The second step is to dissolve again. The degummed silk is quickly placed in a fresh 9.3 mol / L lithium bromide solution to control the final silk protein concentration to 10 w / v%. The solution is centrifuged at 8000 rpm for 10 minutes to remove bubbles. The clear liquid is drawn into a MWCO3500 dialysis bag and dialyzed with ultrapure water for 2 days, during which the water is changed 6 times. The silk protein obtained is diluted to 1% with ultrapure water.
[0133] 2) The preparation of the silk protein framework is the same as in Example 1, the preparation of the ceramic precursor mother solution is the same as in Example 2, and the preparation of the hydroxyapatite-silk protein-mimic Haversian tube structure ceramic-based material is the same as in Example 2. In this material, the mass ratio of the chitin framework to the hydroxyapatite is approximately 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0134] Example 4
[0135] This embodiment provides a silicon dioxide-chitin-haverd tube structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0136] 1) The preparation of chitin framework is the same as that in Example 1.
[0137] 2) Preparation of ceramic precursor mother solution: Measure 100 mL of tetraethyl silicate precursor solution (concentration is 2 wt%), and adjust the pH to 8.5 with 1 M sodium hydroxide solution; or adjust the pH to 5.5 with 1 M hydrochloric acid.
[0138] The preparation of the silica-chitin-mimicking Haversian tube structure ceramic-based material is the same as that in Example 2. In this material, the mass ratio of the chitin framework to the silica is approximately 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0139] Example 5
[0140] This embodiment provides a barium carbonate-chitin-haverd tube-like structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0141] 1) The preparation of chitin framework is the same as that in Example 1.
[0142] 2) Preparation of ceramic precursor mother solution: Weigh 10 grams of barium carbonate powder and add it to 1L ultrapure water, stir it in a constant temperature water tank at 25℃ for 4 hours, and continuously introduce carbon dioxide (flow rate of one bubble per second). Then filter the solution to remove the suspended barium carbonate (final barium ion concentration 10mM). Take 400mL of the supernatant and add magnesium chloride (final concentration 24mM) and polyacrylic acid (final concentration 0.6mM).
[0143] 3) The barium carbonate-chitin-mimic Haversian tube structure ceramic-based material is the same as that in Example 1. In this material, the mass ratio of the chitin framework to the barium carbonate is 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0144] Example 6
[0145] This embodiment provides a titanium dioxide-chitin-haverd tube structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0146] 1) The preparation of chitin framework is the same as that in Example 1.
[0147] 2) Preparation of ceramic precursor mother solution: Tetrabutyl titanate solution and deionized water were mixed according to the ratio, and the concentration of tetrabutyl titanate in the ceramic precursor mother solution was controlled to be 2wt%, and then the pH of the solution was adjusted to 7-8, and polyacrylic acid (molecular weight 1800, final concentration 0.6mM) was added.
[0148] 3) The preparation of titanium dioxide-chitin-mimic Haversian tube structure ceramic-based material is the same as that in Example 1. In this material, the mass ratio of chitin framework to titanium dioxide is 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0149] Example 7
[0150] This embodiment provides a calcium carbonate-gelatin-haver tube structure ceramic-based material, and the preparation method is carried out according to the following steps:
[0151] 1) Preparation of gelatin solution: 2 g of gelatin powder (Sigma) was weighed into a 200 mL beaker, and 98 mL of deionized water was added. The mixture was stirred vigorously (300 rpm) and heated to 90° C. to obtain a uniform 2 w / v% (20 mg / mL) gelatin solution.
[0152] 2) The preparation method of the gelatin frame is the same as that in Example 1, the configuration of the ceramic precursor mother liquid is the same as that in Example 1, and the preparation of the calcium carbonate-gelatin-mimic Haversian tube structure ceramic-based material is the same as that in Example 1. In this material, the mass ratio of the gelatin frame to calcium carbonate is 1:1, the length of the through hole is 15 mm, the pore diameter is 1 mm, the spacing between the through holes is 2 mm, the average pore diameter of the micropores is 1 to 20 μm, and the length of the micropores is 2 mm.
[0153] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A porous ceramic material with a cross-scale Haversian tube structure. It is characterized in that It comprises a plurality of Haversian tube-like structural units; the Haversian tube-like structural units are composed of an organic carrier and a ceramic loaded on the organic carrier; The organic carrier has a multi-level pore structure; The multi-level holes include through holes and micro holes; The through holes and micro holes are in different directions; The through hole has a larger diameter than the micropore; The mass ratio of the organic carrier to the ceramic is 1:(0.1-2); The through hole has a diameter of ≥400 μm and a length of >100 μm; The average pore size of the micropores is ≤100 μm, and the length is >10 μm; The method for preparing the porous ceramic material with a cross-scale Haversian tube-like structure comprises: a. contacting the organic solution with a metal mold, freezing the metal mold, and removing the metal mold to obtain an organic carrier; b. mixing the organic carrier obtained in step a with the ceramic precursor mother solution, and performing in-situ growth to obtain a porous ceramic material with a cross-scale Haversian tube-like structure; The metal mold includes a receiving cavity for carrying a coolant and a forming column group arranged at the outer bottom of the receiving cavity; The forming column group includes a plurality of forming columns.
2. The porous ceramic material with a cross-scale Haversian tube structure according to claim 1, It is characterized in that The micropores are distributed around the through holes; the through holes are interconnected with the micropores.
3. The porous ceramic material with a cross-scale Haversian tube structure according to claim 2, It is characterized in that The aperture of the micropores on the side close to the through hole is small, and the aperture of the micropores on the side away from the through hole is large.
4. The porous ceramic material with a cross-scale Haversian tube structure according to claim 1, It is characterized in that The number of the Haversian tube-like structural units is 1 to 50.
5. The porous ceramic material with a cross-scale Haversian tube structure according to claim 1, It is characterized in that The organic carrier includes one or more of a silk protein framework, a sodium alginate framework, a polyvinyl alcohol framework, a collagen framework, a chitin framework, a gelatin framework, and a sodium polystyrene sulfonate framework; The ceramic is one or more of calcium carbonate, barium carbonate, hydroxyapatite, silicon dioxide, iron oxide, aluminum oxide, titanium oxide, zirconium oxide, silicon oxide, silicon carbide, and boron nitride; The particle size of the ceramic is 10-200 nm.
6. The porous ceramic material of the cross-scale Haversian tube-like structure according to claim 1, wherein the metal mold comprises a receiving cavity for carrying a coolant and a forming column group arranged at the outer bottom of the receiving cavity; The forming column group includes a plurality of forming columns.
7. The porous ceramic material with a cross-scale Haversian tube-like structure according to claim 6, It is characterized in that The molded columns are distributed in an array; The gap between adjacent molding columns is >10μm; The length of the molded column is >100 μm and the diameter is >400 μm.
8. A method for preparing a porous ceramic material with a cross-scale Haversian tube structure. It is characterized in that include: a. contacting the organic solution with the metal mold according to claim 6 or 7, freezing the metal mold, and removing the metal mold to obtain an organic carrier; b. mixing the organic carrier obtained in step a with the ceramic precursor mother solution, and performing in-situ growth to obtain a porous ceramic material with a cross-scale Haversian tube-like structure; The organic solution includes one or more of a silk protein solution, a sodium alginate solution, a polyvinyl alcohol solution, a collagen solution, a chitin solution, a gelatin solution, and a sodium polystyrene sulfonate solution.
9. The method for preparing the porous ceramic material with a cross-scale Haversian tube-like structure according to claim 8, It is characterized in that The temperature of mixing the organic carrier and the ceramic precursor mother solution is 40-50° C. and the time is greater than 12 days; The ceramic precursor is one or more of a calcium carbonate precursor, a barium carbonate precursor, a hydroxyapatite precursor, a silicon dioxide precursor, an iron oxide precursor, an aluminum oxide precursor, a titanium oxide precursor, a zirconium oxide precursor, a silicon oxide precursor, a silicon carbide precursor, a boron nitride precursor, tetrabutyl titanate, and tetraethyl silicate; The particle size of the ceramic precursor is 5-25 nm; The concentration of the organic solution is 1-4 w / v%.