N-type conductive silver paste and preparation method thereof

By combining specific components of glass powder and lead powder with a preferred organic binder, an N-type conductive silver paste was prepared, which solved the problem of increased contact resistance caused by excessive aluminum powder, improved the photoelectric conversion efficiency and heat resistance of solar cells, and is suitable for industrial production.

CN116612915BActive Publication Date: 2024-11-08NANTONG T SUN NEW ENERGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310717894.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-16
Publication Date
2024-11-08
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

Excessive aluminum powder content in existing conductive pastes leads to increased contact resistance, affecting the photoelectric conversion efficiency of solar cells. Furthermore, improper selection of glass powder components in traditional conductive pastes can cause contact resistance and corrosion problems.

Method used

By using a combination of main glass and auxiliary glass with specific components, and by replacing part of the aluminum powder with an appropriate amount of lead powder, and by using lead powder with a specific particle size and a preferred organic binder, an N-type conductive silver paste is prepared. This improves the sintering effect and reduces the carrier recombination rate, thereby reducing the contact resistance.

Benefits of technology

It achieves lower contact resistance and higher fill factor, improves the photoelectric conversion efficiency of solar cells, and maintains good heat resistance and corrosion resistance, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004289977830000091
    Figure BDA0004289977830000091
  • Figure BDA0004289977830000092
    Figure BDA0004289977830000092
  • Figure BDA0004289977830000101
    Figure BDA0004289977830000101
Patent Text Reader

Abstract

The present invention belongs to the field of solar cells, and in particular to the field of H01B1 / 22, and more specifically to an N-type conductive silver paste and a preparation method thereof, wherein the raw materials for preparation thereof at least include, by weight, 80-90 parts of silver powder, 2.1-4.5 parts of glass powder, 1-2 parts of aluminum powder, 0.1-0.8 parts of lead powder, and 5-10 parts of organic binder, and the preparation method is to place the raw materials for preparation on a three-roll grinder for slurry rolling. The N-type conductive silver paste prepared by the present invention has not only a lower contact resistance, but also a higher filling factor, and can improve the photoelectric conversion efficiency of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of solar cells, in particular to the field of H01B1 / 22, and more specifically to an N-type conductive silver paste and a preparation method thereof. Background Art

[0002] As a green and clean energy, solar energy is gaining more and more attention due to its wide sources and large total amount. With the continuous decrease in the total amount of non-renewable resources such as oil and coal, the proportion of solar energy in the energy currently used by humans is increasing. How to efficiently utilize solar energy is actively studied by countries around the world. The utilization of solar energy mainly includes two main methods: photothermal and photoelectric conversion. Among them, solar cells are mainly based on photoelectric conversion. Solar cells can be divided into crystalline silicon cells and thin-film cells. Crystalline silicon solar cells are mainly prepared with high-purity single crystal silicon as the main raw material, so they have a high photoelectric conversion efficiency. Conductive paste is one of the main raw materials of silicon-based solar cells. Silicon-based solar cells generally print the conductive paste on the crystalline silicon substrate by screen printing and other methods, and then prepare the electrode by firing. Common raw materials for preparing conductive paste include organic solvents, metal powders, glass powders and organic carriers.

[0003] Prior art is that the patent CN115832073A discloses a crystalline silicon solar cell back field passivation aluminum conductive paste and a preparation method, the raw materials for preparing the aluminum conductive silver paste mainly include modified aluminum powder, organic adhesive, auxiliary agent, glass powder, etc., the conductive silver paste can effectively reduce the carrier recombination rate, improve the carrier collection rate, so that the solar cell has a higher photoelectric conversion efficiency; Prior art is that the patent CN104575685A discloses a crystalline silicon solar cell high adhesion back field aluminum conductive paste and a preparation method, the raw materials for preparing the crystalline silicon solar cell mainly include aluminum powder, glass powder, organic adhesive, auxiliary agent, wherein the glass powder mainly includes aluminum oxide, silicon dioxide, zinc oxide, boron oxide, etc., the conductive paste is not only low in cost, but also produces less pollutants. However, the glass powder in the above conductive paste contains more aluminum powder, and the aluminum oxide particles in the molten state can move freely to achieve the effect of conductivity, but if the amount of aluminum powder is large, the contact resistance of the conductive paste will also increase, which will affect the photoelectric conversion efficiency of the solar cell to a certain extent. Therefore, how to develop a conductive paste with lower static resistance to improve the photoelectric conversion efficiency of crystalline silicon solar cells has become a hot research topic. Summary of the invention

[0004] In order to solve the above problems, the first aspect of the present invention provides an N-type conductive silver paste, the preparation raw materials of which include at least 80-90 parts of silver powder, 2.1-4.5 parts of glass powder, 1-2 parts of aluminum powder, 0.1-0.8 parts of lead powder, and 5-10 parts of organic binder in terms of mass fractions.

[0005] The silver powder in the present invention can be one or more of monodisperse spherical silver powder, non-monodisperse spherical silver powder, linear silver powder, flaky silver powder, rod-shaped silver powder, and star-shaped silver powder, among which the monodisperse spherical silver powder can improve the fluidity of the conductive paste, reduce the shrinkage rate during the sintering process, and has good sintering activity; the present application does not limit the specific form of the silver powder.

[0006] Preferably, the raw material for preparing the glass powder includes lead oxide.

[0007] Preferably, the glass powder includes main glass and auxiliary glass;

[0008] Further preferably, the mass fraction of the main glass is 2-4 parts, and the mass fraction of the auxiliary glass is 0.1-0.5 parts.

[0009] Further preferably, the raw materials for preparing the main glass and / or the auxiliary glass include lead oxide.

[0010] Preferably, the raw materials for preparing the main glass include at least 15 to 25 parts of lead oxide and 10 to 15 parts of boron oxide in terms of mass percentage; the raw materials for preparing the main glass also include at least one or more of copper oxide and titanium oxide.

[0011] Preferably, the raw materials for preparing the auxiliary glass include at least 30 to 45 parts of lead oxide and 25 to 30 parts of boron oxide in terms of mass percentage; the raw materials for preparing the auxiliary glass also include at least one or more of cobalt oxide, nickel oxide, and chromium oxide.

[0012] In the present invention, main glass and auxiliary glass of specific components are selected and compounded in N-type conductive silver paste, wherein the raw materials for preparing the main glass include at least 15 to 25 parts of lead oxide and 10 to 15 parts of boron oxide by weight, and may also include one or more of copper oxide and titanium oxide; the raw materials for preparing the auxiliary glass include at least 30 to 45 parts of lead oxide, 25 to 30 parts of boron oxide, and 1 to 5 parts of zinc oxide by weight; and may also include one or more of cobalt oxide, nickel oxide, and chromium oxide. Since the compounded raw materials have a more suitable thermal expansion coefficient and wettability, they can promote the wetting of metal aluminum powder and lead powder, and can be better sintered in the conductive silver paste. In addition, the main glass and the auxiliary glass have a more suitable thermal expansion coefficient and wettability after compounding. Glass can etch the anti-reflection layer, promote the contact between the slurry and the silicon wafer to have a better bonding effect, the glass powder begins to soften after sintering to the softening point, the main glass and the auxiliary glass have complementary functions, which can reduce the carrier recombination rate, thereby reducing the contact resistance and improving the photoelectric conversion efficiency of the battery; if the amount of the main glass and the auxiliary glass added is small, it will affect the conductive properties of the slurry. If the amount added is large, the lead boron component itself has a certain corrosiveness and will corrode the Poly layer of the battery, which will cause the contact resistance to increase. Only when the mass percentage of the main glass in the N-type conductive silver paste is 2-4% and the mass percentage of the auxiliary glass in the N-type conductive silver paste is 0.1-0.5% in this system, can the N-type conductive silver paste have better conductive properties.

[0013] Preferably, the D50 particle size of the lead powder is 1.5-3 μm.

[0014] Further preferably, the lead powder has a D10 particle size of 1.0-1.3 μm, a D50 particle size of 2.0-3.0 μm, a D90 particle size of 4.0-5.0 μm, a D98 particle size of 5.1-6.5 μm, and a D100 particle size of 6.6-9.0 μm.

[0015] Preferably, the mass ratio of the silver powder to the aluminum powder is (85-90):(1-2).

[0016] Further preferably, the mass ratio of the aluminum powder to the lead powder is (3-5):(1-1.3).

[0017] As an implementable example, the mass ratio of the aluminum powder to the lead powder may include 3:1, 4:1, 5:1 or 4:1.25.

[0018] Aluminum powder is used as one of the main raw materials for preparing conductive paste for solar cells because of its specific metallic luster and shielding function, as well as excellent heat resistance, water resistance and corrosion resistance, and low cost. However, due to the high resistivity of aluminum powder, which is about 2.65×10 -8Ω·m, if the content is too much, the static resistance of the conductive paste will be significantly increased. The inventors have found that when a small amount of lead powder, especially D10 particle size of 1.0-1.3μm, D50 particle size of 2.0-3.0μm, D90 particle size of 4.0-5.0μm, D98 particle size of 5.1-6.5μm, D100 particle size of 6.6-9.0μm, is used to replace part of the aluminum powder, the situation of excessive static resistance of the conductive silver paste can be significantly improved. The resistivity of lead powder is significantly lower than that of aluminum powder. At the same time, lead powder also has excellent conductivity, can replace part of the aluminum powder, while maintaining the level of contact resistance, reduce line resistance, thereby improving the filling factor, and lead powder of a specific particle size can also improve the capacity and conductivity of solar cells, improve the impact resistance, heat resistance and corrosion resistance of the battery, and make the battery more stable. When the glass powder contains lead oxide, the addition of lead powder can also balance the reaction between lead oxide and silver, improve the sintering effect, and reduce the contact resistance. When the mass ratio of aluminum powder to lead powder is (3-5): (1-1.3), the conductive silver paste has better conductivity and corrosion resistance. However, when the lead powder content is too high, the conductive efficiency will be reduced. The inventors speculate that if the lead content is too high, solid lead compound precipitation will be produced during use, resulting in increased static resistance. In addition, the lead element is highly toxic to the human body. Using too much lead powder will have a significant impact on human health and safety.

[0019] Preferably, the raw materials for preparing the organic adhesive include a carrier and a solvent.

[0020] Preferably, the carrier includes at least one of polymethacrylamide, rosin resin, SEPS, PVB resin, ethyl cellulose, polyvinyl butyral, acrylic resin, cellulose acetate butyrate resin, SEBS, and SBS.

[0021] Further preferably, the carrier is polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose; the mass ratio of polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose is (3-8):(3-5):(5-9):(5-10):(1-2); as an implementable case, the mass ratio of polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose may include 6:5:7:8:2, 3:3:5:5:1 or 8:5:9:10:2.

[0022] Preferably, the solvent includes at least one of cyclohexanone, butyl carbitol, abietol, butyl carbitol acetate, diethylene glycol diethyl ether, dimethyl adipate, and dodecanoate.

[0023] More preferably, the solvent includes butyl carbitol acetate and abietol.

[0024] Further preferably, the mass ratio of butyl carbitol acetate and diethylene glycol diethyl ether is (1-1.5):1; as an implementable case, the mass ratio of butyl carbitol acetate and diethylene glycol diethyl ether may include 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1.

[0025] Further preferably, the mass ratio of the carrier to the solvent is (3-5):1; as an implementable case, the mass ratio of the carrier to the solvent may include 3:1, 4:1 or 5:1.

[0026] In the present invention, the carrier includes polymethacrylamide, rosin resin, PVB resin, and ethyl cellulose, wherein the polymethacrylamide can significantly enhance the dispersibility of the system, the rosin resin can prevent the silver conductive paste from further deepening its oxidation degree during the drying process, the PVB resin can modify the SEPS, and cooperate with the SEPS to make the mechanical properties of the conductive silver paste more excellent, and the ethyl cellulose can increase the viscosity of the system and promote the adhesion between the conductive paste and the silicon wafer to be more excellent. When the mass ratio of polymethacrylamide, rosin resin, SEPS, PVB resin, and ethyl cellulose is ( 3-8):(3-5):(5-9):(5-10):(1-2), it has better stability and bonding performance, is not easy to volatilize, has good rheological properties, has a high boiling point, and has low toxicity. It can quickly solidify, so that the viscosity of the slurry is moderate, the fluidity is good, the adhesion is strong, the contact between the various prepared raw materials is closer, and it is easy to form a dense silver film during screen printing, and the resistivity of the film is small, which further improves the photoelectric conversion efficiency of the photovoltaic cell and increases the service life of the battery. In addition, the above-mentioned carrier can be completely volatilized after sintering, and very little ash is generated, which basically does not affect the performance of the battery.

[0027] As an implementable example, the N-type conductive silver paste may further include one or more functional additives, such as a leveling agent, a defoaming agent, a stabilizer, an anti-aging agent, and the like.

[0028] Preferably, the method for preparing the organic adhesive comprises: dissolving the carrier in a solvent, and heating to 110-140° C. until the carrier is completely dissolved, thereby obtaining the organic adhesive.

[0029] As an implementable example, the heating temperature may include 110°C, 120°C, 125°C, 130°C or 140°C.

[0030] The second aspect of the present invention provides a method for preparing an N-type conductive silver paste: silver powder, glass powder, aluminum powder, lead powder and an organic binder are placed in a three-roll grinder for slurry rolling to obtain an N-type conductive silver paste.

[0031] Beneficial Effects

[0032] (i) In the present invention, by using specific preparation raw materials including 80-90 parts of silver powder, 2.1-4.5 parts of glass, 1-2 parts of aluminum powder, 0.1-0.8 parts of lead powder, and 5-10 parts of organic binder, the N-type conductive silver paste prepared not only has a lower contact resistance, but also has a higher filling factor, so that the photoelectric conversion efficiency of the solar cell is improved to a certain extent.

[0033] (ii) The glass powder in the present invention is a composite of main glass and auxiliary glass of specific components, and the conductive functions of the two are complementary, which can reduce the carrier recombination rate, thereby reducing the contact resistance and improving the photoelectric conversion efficiency; when the glass powder includes lead oxide, the addition of lead powder can balance the reaction between the lead oxide and silver powder in the glass powder, improve the sintering effect, and reduce the contact resistance.

[0034] (III) In the present invention, by limiting the mass ratio of aluminum powder to lead powder to (3-5): (1-1.3), not only the resistance value of N-type conductive silver paste can be reduced, but also the heat resistance, water resistance and corrosion resistance of the conductive silver paste will not be significantly affected. Moreover, lead powder can replace part of aluminum powder, while maintaining the level of contact resistance, reducing line resistance, thereby improving fill factor.

[0035] (IV) In the present invention, when the carrier includes polymethacrylamide, rosin resin, SEPS, PVB resin, and ethyl cellulose in a mass ratio of (3-8): (3-5): (5-9): (5-10): (1-2), the N-type conductive silver paste has better stability and bonding performance, strong adhesion, and the contact between the prepared raw materials is closer.

[0036] (V) The preparation method of the N-type conductive silver paste in the present invention is relatively simple, and only requires mixing the various prepared raw materials and rolling the slurry, which is suitable for industrial scale-up production. DETAILED DESCRIPTION

[0037] Example 1

[0038] In a first aspect, the present embodiment provides an N-type conductive silver paste, wherein the raw materials for preparing the paste are as follows by weight: 86.45 parts of silver powder, 3.3 parts of glass powder, 1 part of aluminum powder, 0.25 parts of lead powder, and 9 parts of organic binder.

[0039] The glass powder comprises 3 parts of main glass and 0.3 parts of auxiliary glass in terms of mass.

[0040] The raw materials for preparing the main glass are calculated by weight: 22 parts of lead oxide, 13 parts of boron trioxide, 20 parts of tellurium dioxide, 7 parts of copper oxide, 18 parts of titanium dioxide, and 20 parts of zinc oxide.

[0041] The raw materials for preparing the auxiliary glass are calculated by weight as follows: 40 parts of lead oxide, 28 parts of boron trioxide, 3 parts of gallium trioxide, 4 parts of manganese dioxide, 7 parts of cobalt oxide, 9 parts of nickel oxide, and 9 parts of chromium trioxide.

[0042] The lead powder has a D10 particle size of 1.216 μm, a D50 particle size of 2.553 μm, a D90 particle size of 4.948 μm, a D98 particle size of 6.299 μm, and a D100 particle size of 8.469 μm.

[0043] The organic adhesive is a carrier and a solvent, and the mass ratio of the carrier to the solvent is 3:1.

[0044] The carrier is polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose, and the weight ratio is 6:5:7:8:2.

[0045] The solvent is butyl carbitol acetate and rosin alcohol, and the mass ratio of butyl carbitol acetate to rosin alcohol is 1.2:1.

[0046] The preparation method of the organic adhesive is as follows: dissolving the carrier in a solvent, heating to 120° C. until the carrier is completely dissolved, thereby obtaining the organic adhesive.

[0047] The second aspect of the present embodiment provides a method for preparing an N-type conductive silver paste, specifically, placing silver powder, glass powder, aluminum powder, lead powder and an organic binder in a three-roll grinder and rolling for three times to obtain an N-type conductive silver paste.

[0048] Example 2

[0049] In a first aspect, the present embodiment provides an N-type conductive silver paste, wherein the raw materials for preparing the paste are as follows, by weight: 85.2 parts of silver powder, 3.3 parts of glass powder, 2 parts of aluminum powder, 0.5 parts of lead powder, and 9 parts of an organic binder.

[0050] The glass powder comprises 3 parts of main glass and 0.3 parts of auxiliary glass in terms of mass.

[0051] The raw materials for preparing the main glass are calculated by weight: 24 parts of lead oxide, 15 parts of boron trioxide, 20 parts of tellurium dioxide, 8 parts of copper oxide, 18 parts of titanium dioxide, and 15 parts of zinc oxide.

[0052] The raw materials for preparing the auxiliary glass are calculated by weight as follows: 40 parts of lead oxide, 30 parts of boron trioxide, 3 parts of gallium trioxide, 4 parts of manganese dioxide, 8 parts of cobalt oxide, 8 parts of nickel oxide, and 7 parts of chromium trioxide.

[0053] The lead powder has a D10 particle size of 1.216 μm, a D50 particle size of 2.553 μm, a D90 particle size of 4.948 μm, a D98 particle size of 6.299 μm, and a D100 particle size of 8.469 μm.

[0054] The carrier is polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose, and the weight ratio is 6:5:7:8:2.

[0055] The solvent is butyl carbitol acetate and rosin alcohol; the mass ratio of butyl carbitol acetate to rosin alcohol is 1.3:1.

[0056] The preparation method of the organic adhesive is as follows: dissolving the carrier in a solvent, heating to 120° C. until the carrier is completely dissolved, thereby obtaining the organic adhesive.

[0057] The second aspect of the present embodiment provides a method for preparing an N-type conductive silver paste, specifically, placing silver powder, glass powder, aluminum powder, lead powder and an organic binder in a three-roll grinder and rolling for three times to obtain an N-type conductive silver paste.

[0058] Example 3

[0059] The specific implementation of this embodiment is the same as that of Embodiment 1, except that the particle size of the lead powder D10 is 1.116 μm; the particle size of D50 is 2.119 μm; the particle size of D90 is 4.2 μm; the particle size of D98 is 5.191 μm; and the particle size of D100 is 6.826 μm.

[0060] Example 4

[0061] The specific implementation of this embodiment is the same as that of Embodiment 2, except that the D10 particle size of the lead powder is 1.116 μm; the D50 particle size is 2.119 μm; the D90 particle size is 4.2 μm; the D98 particle size is 5.191 μm; and the D100 particle size is 6.826 μm.

[0062] Comparative Example 1

[0063] In a first aspect of the present comparative example, an N-type conductive silver paste is provided, and the raw materials for preparing the paste are as follows, by weight: 85.7 parts of silver powder, 3.3 parts of glass powder, 1 part of aluminum powder, and 9 parts of organic binder.

[0064] The glass powder comprises 3 parts of main glass and 0.3 parts of auxiliary glass in terms of mass.

[0065] The raw materials for preparing the main glass are, by weight, 22 parts of lead oxide, 13 parts of boron trioxide, 20 parts of tellurium dioxide, 7 parts of copper oxide, 18 parts of titanium dioxide, and 20 parts of zinc oxide.

[0066] The raw materials for preparing the auxiliary glass are calculated by weight as follows: 40 parts of lead oxide, 28 parts of boron trioxide, 3 parts of gallium trioxide, 4 parts of manganese dioxide, 7 parts of cobalt oxide, 9 parts of nickel oxide, and 9 parts of chromium trioxide.

[0067] The lead powder has a D10 particle size of 1.216 μm, a D50 particle size of 2.553 μm, a D90 particle size of 4.948 μm, a D98 particle size of 6.299 μm, and a D100 particle size of 8.469 μm.

[0068] The organic adhesive is a carrier and a solvent, and the mass ratio of the carrier to the solvent is 3:1.

[0069] The carrier is polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose, and the weight ratio is 6:5:7:8:2.

[0070] The solvent is butyl carbitol acetate and rosin alcohol, and the mass ratio of butyl carbitol acetate to rosin alcohol is 1.2:1.

[0071] The preparation method of the organic adhesive is as follows: dissolving the carrier in a solvent, heating to 120° C. until the carrier is completely dissolved, thereby obtaining the organic adhesive.

[0072] The second aspect of the present comparative example provides a method for preparing an N-type conductive silver paste, specifically, placing silver powder, glass, aluminum powder, lead powder and an organic binder in a three-roll grinder and rolling for three times to obtain an N-type conductive silver paste.

[0073] Comparative Example 2

[0074] The first aspect of the present comparative example provides an N-type conductive silver paste, and the raw materials for preparing the paste are as follows in percentage by mass: 86.7 parts of silver powder, 3.3 parts of glass powder, 1 part of aluminum powder, and 9 parts of organic binder.

[0075] The glass powder comprises 3 parts of main glass and 0.3 parts of auxiliary glass in terms of mass.

[0076] The raw materials for preparing the main glass are, by weight, 22 parts of lead oxide, 13 parts of boron trioxide, 20 parts of tellurium dioxide, 7 parts of copper oxide, 18 parts of titanium dioxide, and 20 parts of zinc oxide.

[0077] The raw materials for preparing the auxiliary glass are calculated by weight as follows: 40 parts of lead oxide, 28 parts of boron trioxide, 3 parts of gallium trioxide, 4 parts of manganese dioxide, 7 parts of cobalt oxide, 9 parts of nickel oxide, and 9 parts of chromium trioxide.

[0078] The organic adhesive is a carrier and a solvent, and the mass ratio of the carrier to the solvent is 3:1.

[0079] The carrier is polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose, and the weight ratio is 6:5:7:8:2.

[0080] The solvent is butyl carbitol acetate and rosin alcohol, and the mass ratio of butyl carbitol acetate to rosin alcohol is 1.2:1.

[0081] The preparation method of the organic adhesive is as follows: dissolving the carrier in a solvent, heating to 120° C. until the carrier is completely dissolved, thereby obtaining the organic adhesive.

[0082] The second aspect of the present embodiment provides a method for preparing an N-type conductive silver paste, specifically comprising: placing silver powder, glass powder, aluminum powder and an organic binder in a three-roll grinder and rolling for three times to obtain an N-type conductive silver paste.

[0083] Performance Evaluation

[0084] 1. Electrical performance test

[0085] Test object: N-type conductive silver paste prepared in Examples 1-4 and Comparative Examples 1-2

[0086] Test method: The client uses a Halm test machine for testing and records the test results in Table 1.

[0087] Table 1

[0088]

[0089] 2. Electrical performance test of conductive silver paste

[0090] Test object: N-type conductive silver paste prepared in Examples 1-4 and Comparative Examples 1-2

[0091] Contact resistance test method: The contact resistance is linearly fitted by TLM method, and the ohmic contact resistance is obtained by inverse calculation of square resistance.

[0092] Fill factor test method: Perform IV (volt-ampere) characteristic curve test on photovoltaic cells, i.e. measure the output power of photovoltaic cells at different voltages and currents by changing the light intensity and circuit load. m ×V m ) / ( Isc ×V oc ). m and V m It is the output current and output voltage of the photovoltaic cell at the maximum output power point (MPP), I sc and V ocare the output current and output voltage of the photocell when short-circuited and open-circuited respectively; the corresponding results are recorded in Table 2.

[0093] Table 2

[0094]

[0095]

Claims

1. An N-type conductive silver paste, characterized in that: The raw materials for its preparation include at least 80-90 parts of silver powder, 2.1-4.5 parts of glass powder, 1-2 parts of aluminum powder, 0.1-0.8 parts of lead powder, and 5-10 parts of organic binder in terms of weight. The raw materials for preparing the glass powder include lead oxide; The mass ratio of the aluminum powder to the lead powder is (3-5): (1-1.3); The mass ratio of the silver powder to the aluminum powder is (85-90): (1-2); The glass powder includes main glass and auxiliary glass; the mass fraction of the main glass is 2-4 parts, and the mass fraction of the auxiliary glass is 0.1-0.5 parts; The raw materials for preparing the main glass include at least 15 to 25 parts of lead oxide and 10 to 15 parts of boron oxide in terms of mass fractions; The raw materials for preparing the main glass also include at least one or more of copper oxide and titanium oxide; The raw materials for preparing the auxiliary glass include at least 30-45 parts of lead oxide and 25-30 parts of boron oxide in terms of mass fractions; The raw materials for preparing the auxiliary glass also include at least one or more of cobalt oxide, nickel oxide and chromium oxide.

2. The N-type conductive silver paste according to claim 1, characterized in that: The D50 particle size of the lead powder is 1.5-3 μm.

3. According to the N-type conductive silver paste of claim 2, the lead powder has a D10 particle size of 1.0-1.3 μm, a D50 particle size of 2.0-3.0 μm, a D90 particle size of 4.0-5.0 μm, a D98 particle size of 5.1-6.5 μm, and a D100 particle size of 6.6-9.0 μm.

4. The N-type conductive silver paste according to claim 1, characterized in that: The raw materials for preparing the organic adhesive include a carrier and a solvent; The carrier at least includes: one or more of polymethacrylamide, rosin resin, SEPS, PVB resin, ethyl cellulose, polyvinyl butyral, acrylic resin, cellulose acetate butyrate resin, SEBS, and SBS.

5. The N-type conductive silver paste according to claim 4, characterized in that: The carrier comprises at least polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose; the mass ratio of polymethacrylamide, rosin resin, SEPS, PVB resin and ethyl cellulose is (3-8): (3-5): (5-9): (5-10): (1-2); and / or the mass ratio of the carrier to the solvent is (3-5):

1.

6. A method for preparing an N-type conductive silver paste according to any one of claims 1 to 5, characterized in that: The method comprises at least the following steps: placing silver powder, glass powder, aluminum powder, lead powder and an organic binder on a three-roll mill to obtain an N-type conductive silver paste.

Citation Information

Patent Citations

  • Crystal silicon solar cell high adhesive force back surface field aluminum electrocondution slurry and preparation method

    CN104575685A

  • Crystalline silicon solar cell back surface field passivation aluminum conductive paste and preparation method thereof

    CN115832073A

  • Positive electrode electrocondution slurry of crystalline silicon solar cell and preparation method therefor

    CN103596648A

  • N-type battery conductive silver paste and preparation method thereof

    CN115410746A

  • Conductive composition

    JP2017092253A