A lithium extraction adsorbent and its preparation method and application

Through the swelling, Fuker alkylation and hydrolysis reaction of macroporous resin with oil-soluble aluminum salt and dichloromethane, a high-performance lithium extract adsorbent is generated, which solves the problems of few active sites and low aluminum load capacity in the prior art. It achieves the effects of fast adsorption speed, large capacity, high selectivity and stable performance.

CN116899525BActive Publication Date: 2024-11-05JIANGSU HELPER FUNCTIONAL MATERIALS
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202311122507.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2024-11-05
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

In the existing lithium extraction technology, the resin-based lithium extracting adsorbent has few active sites and low aluminum load capacity, resulting in low lithium extracting adsorbent activity, exchange rate and lithium extracting capacity.

Method used

After swelling with macroporous resin, oil-soluble aluminum salt and dichloromethane, the lithium extracting adsorbent with high selectivity and high adsorption capacity is generated by Fuker alkylation reaction and hydrolysis. Aluminum chloride is used as a catalyst and reaction medium to increase aluminum Loading rate and resin properties.

Benefits of technology

The lithium-extracting adsorbent is achieved with fast adsorption speed, large adsorption capacity, high selectivity, stable performance and long service life. The reaction steps are simplified, the reaction costs are reduced, and the aluminum loading rate is increased.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116899525B_ABST
    Figure CN116899525B_ABST
Patent Text Reader

Abstract

The present invention discloses a lithium extraction adsorbent and its preparation method and application, comprising the following steps: (1) swelling: mixing a macroporous resin with dichloromethane and an oil-soluble aluminum salt, stirring and swelling for a period of time; (2) Friedel-Crafts alkylation reaction: adding aluminum chloride to the reaction system of step (1), stirring, and then heating and refluxing for reaction. After the reaction is completed, dichloromethane is recovered by distillation, and the resin is washed with hot water; (3) hydrolysis: mixing the hydrolysis solution with the resin washed in step (2), heating and refluxing for reaction, washing, and obtaining a lithium extraction adsorbent. The present invention utilizes dichloromethyl alkylation and aluminum chloride to hydrolyze at the same time, and uses the polar groups after hydrolysis to anchor the amorphous aluminum hydroxide ion sieve. The present invention can overcome the problems of less active sites in the direct embedding method in the existing resin-based lithium extraction adsorbent technology, and low aluminum loading capacity in the resin hybridization reaction, which ultimately leads to low activity, exchange rate and lithium extraction capacity of the lithium extraction adsorbent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of adsorbents, and in particular relates to a lithium extraction adsorbent and a preparation method and application thereof. Background Art

[0002] As the metal element with the lowest molecular weight in nature, lithium has excellent electrochemical activity and is widely used in energy, chemical industry, metallurgy, medicine, electronics and other fields. It is known as "industrial MSG". Lithium cannot be replaced in most applications. my country's lithium salt lake resources are mainly distributed in Qinghai Province and Tibet Autonomous Region. Among them, Qinghai Province accounts for nearly 50% of the lithium resource reserves, and Tibet Autonomous Region accounts for 30%. Because the physical and chemical properties of magnesium and lithium are very similar, it is very difficult to separate magnesium and lithium. Since the magnesium-lithium ratio of most salt lake brines in my country is high, the magnesium-lithium ratio is further increased after the original brine is extracted with potassium through traditional processes, the lithium extraction technology is more difficult, and the lithium extraction rate is low.

[0003] The main methods for extracting lithium from salt lake brine include solvent extraction, adsorption, membrane separation, electrochemical method, reaction / separation coupling technology, etc. Among them, liquid-liquid extraction technology has the advantages of simple process, easy to control operating conditions, low cost, high extraction efficiency and selectivity. It is considered to be the most outstanding method in terms of ion selectivity and lithium yield in Qinghai salt lake brine lithium extraction technology. However, the environmental problems of the extractant and the high requirements for extraction equipment have restricted the industrial application of this technology to a certain extent. The membrane separation method is costly and not easy to industrialize. The electrochemical method can avoid the use of acid to wash the material during the lithium removal process, thereby reducing material dissolution and enhancing the cycle performance. It is a low-energy, high-efficiency lithium extraction technology, but the chemical reaction on the electrode needs to avoid side reactions, and the electrolyte composition requirements are high. The system needs to be further optimized and has not yet been mass-produced. The adsorption method is a lithium extraction technology with great advantages from the environmental and economic perspectives, especially the advantages of extracting lithium from low-grade high-magnesium lithium brines and seawater. Obviously, for my country's low-grade salt lakes, the adsorption method is the most promising method.

[0004] The core of the adsorption method is to prepare lithium adsorbents with high selectivity, large adsorption capacity and good cycle stability. In recent years, most of the research reports on lithium extraction by adsorption method use inorganic adsorbents, mainly ion sieve oxides and aluminum adsorbents. Among them, ion sieve oxides include manganese ion sieves, titanium ion sieves and doped ion sieves. Manganese adsorbents are the research hotspot of lithium ion sieve adsorbents. They are spinel structures, mainly LiMn2O4, Li4Mn5O 12 , Li 1.6 Mn 1.6 O4, etc., lithium manganese oxide is acid-leached, Li + H +The expression of aluminum adsorbent is "LiCl·mAl(OH)3·nH2O" (Li / Al-LDHs), where LiCl is inserted into the amorphous Al(OH)3 interlayer and Li + Enter into the Al-O octahedral vacancy and deintercalate some Li + After that, the aluminum adsorbent has steric hindrance effect and memory effect, thereby selectively adsorbing Li + After adsorption saturation, it is eluted with water, without introducing other impurities, and the operating cost is low. However, this type of adsorbent is usually formed by co-precipitation of crystals aggregated into unstable particles, mostly in powder form, with poor mechanical strength and high dissolution rate. For this reason, it is usually necessary to granulate this type of adsorbent.

[0005] There are multiple patent reports using monomers to polymerize resins in situ, directly embedding lithium adsorbents to form granulation. Patent CN104014308A uses monomers to polymerize resins to directly embed aluminum hydroxide powder, which improves the loading rate and adsorption capacity of active inorganic particles to 14mg / g. Patent CN102631897A also uses similar binders for embedding, and its molecular sieve type or ion sieve type lithium adsorbent uses insoluble hydroxides, with an exchange capacity of 3-15mg / ml (resin). CN106975436A uses chlorine-containing polymers (such as vinyl chloride) powders and aluminum hydroxide to mix, and adds liquid chlorine to soften the embedding skeleton during extrusion. Although this method can make the resin have a larger specific surface area by pore making, the inorganic particle surface interface is closely combined with the resin after embedding, and the exposed surface is still small, and the aluminum hydroxide powder is smaller than the surface itself, so the exchange rate and lithium extraction capacity are still low.

[0006] Another resin hybrid method is to first enrich aluminum ions in the resin pores, and then precipitate aluminum hydroxide in the pores. U.S. Patent US4221767 discloses a method of loading LiCl·2Al(OH)3·nH2O on anion exchange resin. The specific method is to first enrich aluminum ions in the resin pores, then precipitate aluminum hydroxide in the pores, then use lithium hydroxide to react with the aluminum hydroxide in the resin, and finally transform it into LiCl·2Al(OH)3·nH2O. This method solves the problem of loading active inorganic particles and maintains its lithium extraction activity, but the pore volume and specific surface area of ​​the anion exchange resin are relatively low. Therefore, the loading amount of active inorganic particles is relatively low, which affects the lithium extraction capacity. Patents CN110237829A and CN111330548A load Al 3+ Porous resin is introduced, and then alkali solution NH3 or NaOH is added to precipitate aluminum hydroxide. The in-situ reaction in the resin has the advantages of open pores and large surface area. 3+The amount introduced is limited, and thus the overall adsorption capacity is limited, wherein the maximum adsorption capacity of the lithium adsorbent prepared in CN111330548A is only 4.1 mg / g. Summary of the invention

[0007] In view of the above-mentioned technical problems, the present invention provides a lithium extraction adsorbent and its preparation method and application. The present invention uses a macroporous resin to adsorb oil-soluble aluminum salt and dichloromethane, and grafts aluminum chloride to the resin through a Friedel-Crafts alkylation reaction to obtain a chloromethylated macroporous resin; then hydrolyzes the resin to obtain a lithium extraction adsorbent. The present invention can overcome the problems of the existing resin-based lithium extraction adsorbent technology, such as the small number of active sites in the direct embedding method and the low aluminum loading capacity in the resin hybridization reaction, which ultimately leads to the problems of low activity, exchange rate and lithium extraction capacity of the lithium extraction adsorbent.

[0008] The technical solution of the present invention is:

[0009] The present invention relates to a method for preparing a lithium extraction adsorbent, comprising the following steps:

[0010] (1) Swelling: Mix the macroporous resin with dichloromethane and oil-soluble aluminum salt, stir and swell for a period of time;

[0011] (2) Friedel-Crafts alkylation reaction: add aluminum chloride to the reaction system of step (1), stir, and then heat and reflux for reaction. After the reaction is completed, recover dichloromethane by distillation, and wash the resin with hot water;

[0012] (3) Hydrolysis: The hydrolysis solution is mixed with the resin washed in step (2), and the mixture is heated to reflux for reaction to hydrolyze the functional groups on the surface of the resin, and then washed to obtain a lithium extraction adsorbent.

[0013] Preferably, in step (1), the macroporous resin is a styrene-based macroporous resin; and the oil-soluble aluminum salt is at least one of aluminum chloride, aluminum nitrate and aluminum sulfate.

[0014] Preferably, in step (1), the mass ratio of the macroporous resin to dichloromethane is 1:3.5-5, and the mass ratio of the oil-soluble aluminum salt to dichloromethane is 1:10-30.

[0015] Preferably, in step (1), the stirring time is 0.5 to 2 hours, and the swelling time is 2 to 12 hours.

[0016] Preferably, the mass ratio of the aluminum chloride added in step (2) to the macroporous resin in step (1) is 0.05 to 0.4:1.

[0017] Preferably, in step (2), the stirring time after adding aluminum chloride is 0.5 to 2 hours;

[0018] In the heating reflux reaction, the heating temperature is 30-40°C and the reflux time is 6-18h;

[0019] The temperature of the hot water used to wash the resin is between 60 and 80°C, and the resin is washed until the supernatant is colorless.

[0020] Preferably, in step (3), the hydrolysis solution is a solution of ammonia water, sodium tetrahydroxyaluminate or a mixed solution of the two, and the mass concentration of the hydrolysis solution is 1 to 10%.

[0021] Preferably, in the heating reflux reaction in step (3), the heating temperature is 20 to 50° C. and the reflux time is 6 to 20 h. The purpose of heating is to accelerate the rate of hydrolysis.

[0022] The present invention also relates to a lithium extraction adsorbent, which is prepared by the above preparation method, and the particle size of the lithium extraction adsorbent is 0.2-0.6 mm. The present invention utilizes dichloromethyl alkylation and simultaneous hydrolysis with aluminum chloride, and uses the polar groups after hydrolysis to anchor the amorphous aluminum hydroxide ion sieve.

[0023] The present invention also relates to the use of the above-mentioned lithium extraction adsorbent in extracting lithium in salt lake brine, wherein the magnesium-lithium mass ratio (Li / Mg) of the salt lake brine is 0.01-1.

[0024] The beneficial effects of the present invention are:

[0025] (1) The present invention utilizes macroporous resin balls to adsorb oil-soluble aluminum salts and dichloromethane, and then performs Friedel-Crafts alkylation reaction to generate benzyl chloromethyl and anchor aluminum chloride, and then hydrolyzes to generate aluminum hydroxide, so that the aluminum content in the resin is high and the aluminum hydroxide density is high. At the same time, the chloromethyl lithium extracting adsorbent has the advantages of fast adsorption speed, large adsorption capacity and high selectivity;

[0026] (2) The lithium extraction adsorbent of the present invention hydrolyzes benzyl chloromethyl to obtain benzyl hydroxyl, which can bond with aluminum hydroxide, so it has stable performance and long service life;

[0027] (3) The oil-soluble aluminum salt used in the present invention has a different function from the aluminum chloride in step (2), wherein the oil-soluble aluminum salt is used to load aluminum into the pores, and the aluminum chloride is used as a catalyst for the Friedel-Crafts reaction; the present invention uses a one-step alkylation reaction, which can simplify the reaction steps, does not introduce other metal ions that interfere with the lithium ion sieve, and can also improve the reaction efficiency and the aluminum loading rate, thereby reducing the reaction cost and improving the resin performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0029] Figure 1 The present invention is a flow chart for preparing the lithium-extracting adsorbent;

[0030] Figure 2 The figure is the X-ray diffraction pattern of the lithium extraction adsorbent of the present invention. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0032] In addition, the styrene-based macroporous resin (particle size 60-100 mesh) used in the following examples was purchased from Shanghai Resin Factory.

[0033] Example 1

[0034] like Figure 1 As shown, a lithium extraction adsorbent and a preparation method thereof specifically include the following steps:

[0035] (1) Swelling: Weigh 100 g of styrene-based macroporous resin, add 400 g of dichloromethane and 40 g of aluminum chloride, stir for 0.5 h, and swell for 2 h;

[0036] (2) Friedel-Crafts alkylation reaction: 20 g of aluminum chloride was then added to the system of step (1), and the mixture was stirred for 0.5 h. The mixture was heated to 40° C. at a rate of 2° C. / min and refluxed for 16 h. The dichloromethane was recovered from the resin after the reaction by distillation, and the residual dichloromethane in the resin was washed with hot water at 80° C.;

[0037] (3) Hydrolysis: Prepare 300 mL of 10% ammonia solution, mix with the resin washed in step (2), heat to 40° C. at 2° C. / min, reflux for 6 h, wash, and obtain the target product.

[0038] Example 2

[0039] A lithium extraction adsorbent and a preparation method thereof, specifically comprising the following steps:

[0040] (1) Swelling: Weigh 100 g of styrene-based macroporous resin, add 400 g of dichloromethane and 25 g of aluminum chloride, stir for 0.5 h, and swell for 2 h;

[0041] (2) Friedel-Crafts alkylation reaction: 25 g of aluminum chloride was then added to the system of step (1), and after stirring for 0.5 h, the temperature was raised to 40° C. at 2° C. / min and refluxed for 16 h. The dichloromethane was recovered from the resin after the reaction by distillation, and the residual dichloromethane in the resin was washed with 80° C. hot water;

[0042] (3) Hydrolysis: Prepare 300 mL of 10% sodium tetrahydroxyaluminate solution, mix with the resin washed in step (2), heat to 40° C. at 2° C. / min, reflux for 6 h, wash, and obtain the target product.

[0043] Example 3

[0044] A lithium extraction adsorbent and a preparation method thereof, specifically comprising the following steps:

[0045] (1) Swelling: Weigh 100 g of styrene-based macroporous resin, add 400 g of dichloromethane and 20 g of aluminum chloride, stir for 0.5 h, and swell for 2 h;

[0046] (2) Friedel-Crafts alkylation reaction: 15 g of aluminum chloride was then added to the system of step (1), and the mixture was stirred for 0.5 h. The mixture was heated to 40° C. at a rate of 2° C. / min and refluxed for 16 h. The dichloromethane was recovered from the resin after the reaction by distillation, and the residual dichloromethane in the resin was washed with hot water at 80° C.;

[0047] (3) Hydrolysis: Prepare 300 mL of 10% sodium tetrahydroxyaluminate solution, mix with the resin washed in step (2), heat to 40° C. at 2° C. / min, reflux for 6 h, wash, and obtain the target product.

[0048] Example 4

[0049] A lithium extraction adsorbent and a preparation method thereof, specifically comprising the following steps:

[0050] (1) Swelling: Weigh 100 g of styrene-based macroporous resin, add 400 g of dichloromethane and 20 g of aluminum sulfate, stir for 0.5 h, and swell for 2 h;

[0051] (2) Friedel-Crafts alkylation reaction: 15 g of aluminum chloride was then added to the system of step (1), and the mixture was stirred for 0.5 h. The mixture was heated to 40° C. at a rate of 2° C. / min and refluxed for 16 h. The dichloromethane was recovered from the resin after the reaction by distillation, and the residual dichloromethane in the resin was washed with hot water at 80° C.;

[0052] (3) Hydrolysis: Prepare 300 mL of 10% sodium tetrahydroxyaluminate solution, mix with the resin washed in step (2), heat to 40° C. at 2° C. / min, reflux for 6 h, wash, and obtain the target product.

[0053] The X-ray diffraction pattern of the lithium extraction adsorbent of the present invention is as follows: Figure 2 As shown, 2θ = 11.5° and 2θ = 24° indicate that the resin material with aluminum hydroxide is successfully synthesized on the surface, and the active inorganic component of the lithium-extracting adsorbent is nAl(OH)3·mH2O, and as Figure 2 As shown, it is a regular layered structure.

[0054] Adsorption process: 1. Take 10mL of material and fill it into a glass chromatography column, then pour in 10BV of brine;

[0055] 2. Carry out the experiment at a rate of 1 BV / h and collect the effluent.

[0056] The adsorption effect of the adsorbent in Examples 1-3 on salt lake brine is shown in Table 1, and the saturated adsorption data for lithium is shown in Table 2.

[0057] Table 1

[0058]

[0059]

[0060] Table 2

[0061]

[0062] It can be seen from Table 1 and Table 2 that the lithium extraction adsorbent prepared by the present invention has a high saturated adsorption capacity for lithium, and has the advantages of fast lithium adsorption speed, large adsorption capacity, high selectivity, stable performance and long service life.

[0063] The dissolution loss rate of the adsorbent in brine adsorption in Examples 1-3 (10 adsorptions) is shown in Table 3 below.

[0064] Table 3

[0065]

[0066] The lithium extraction adsorbent prepared by the method of the present invention can fundamentally solve the shortcomings of poor mechanical strength, high dissolution rate, low activity, etc. when active inorganic lithium extraction particles (nAl(OH)3·mH2O) are used as lithium extraction adsorbents.

[0067] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for preparing a lithium extraction adsorbent, characterized in that: The following steps are involved: (1) Swelling: Mix a macroporous resin with dichloromethane and an oil-soluble aluminum salt, stir and swell for a period of time; wherein the macroporous resin is a styrene-based macroporous resin; the oil-soluble aluminum salt is aluminum sulfate; the mass ratio of the macroporous resin to dichloromethane is 1:4, and the mass ratio of aluminum sulfate to dichloromethane is 1:20; (2) Friedel-Crafts alkylation reaction: aluminum chloride is added to the reaction system of step (1), stirred, and then heated to reflux for reaction. After the reaction is completed, dichloromethane is recovered by distillation, and the resin is washed with hot water; the mass ratio of aluminum chloride added in step (2) to the macroporous resin in step (1) is 0.15:1; (3) Hydrolysis: Using sodium tetrahydroxyaluminate with a mass concentration of 10% as a hydrolysis solution, the hydrolysis solution is mixed with the resin washed in step (2), the mixture is heated to reflux for reaction, and then washed to obtain a lithium extraction adsorbent.

2. The method for preparing a lithium extraction adsorbent according to claim 1, characterized in that: In step (1), the stirring time is 0.5 to 2 hours, and the swelling time is 2 to 12 hours.

3. The method for preparing a lithium extraction adsorbent according to claim 1, characterized in that: In step (2), the stirring time after adding aluminum chloride is 0.5 to 2 hours; In the heating reflux reaction, the heating temperature is 30-40°C and the reflux time is 6-18h; The temperature of the hot water used to wash the resin is between 60 and 80°C, and the resin is washed until the supernatant is colorless.

4. The method for preparing a lithium extraction adsorbent according to claim 1, characterized in that: In the heating reflux reaction in step (3), the heating temperature is 20 to 50° C. and the reflux time is 6 to 20 h.

5. A lithium extraction adsorbent, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the lithium extraction adsorbent according to claim 5 in extracting lithium from salt lake brine, wherein the magnesium-lithium mass ratio of the salt lake brine is 0.01 to 1.

Citation Information

Cited By

  • Adsorption lithium extraction method and adsorption lithium extraction device

    CN121137379A

  • Method for lithium extraction by adsorption and apparatus for lithium extraction by adsorption

    CN121137379B

  • Spherical-like high-adsorption-capacity high-strength lithium extraction adsorbent and preparation method thereof

    CN121732113A

  • Fresh water-saving brine lithium extraction method

    CN121976059A