Mica paper treatment liquid, mica paper, mica board and preparation method and application thereof

By treating mica paper with specific ratios of silicone gel, aluminum nitride powder, wollastonite and silane coupling agent, hot pressing and composite, combined with insulating coating treatment liquid, the problem of insufficient insulation and insulation performance of mica boards is solved, and the problem of Efficient heat insulation and high-temperature insulation performance improve, meeting the needs of new energy vehicles.

CN117230653BActive Publication Date: 2024-11-22BEIJING YITIAN MICA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311232709.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-22
Publication Date
2024-11-22
Estimated Expiration
2043-09-22

AI Technical Summary

Technical Problem

The existing mica boards cannot meet the requirements of high heat insulation and high temperature insulation performance in thermal runaway protection materials for power batteries of new energy vehicles, and there are problems of poor thermal insulation and insufficient insulation.

Method used

Mica paper treatment liquid is prepared using specific ratios of silicone gel, aluminum nitride powder, wollastonite and silane coupling agents, and the mica paper is processed and combined by hot pressing to form a mica board, and the surface of the mica board is coated with insulating coating. The layer treatment liquid is used to improve its thermal insulation and high temperature insulation properties.

Benefits of technology

It realizes excellent thermal insulation and high-temperature insulation performance of mica boards, can meet the requirements of thermal runaway protective materials for power batteries of new energy vehicles, has good adhesive performance and insulation effect, and avoids layering and glue spilling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004464468120000061
    Figure BDA0004464468120000061
  • Figure BDA0004464468120000071
    Figure BDA0004464468120000071
  • Figure BDA0004464468120000072
    Figure BDA0004464468120000072
Patent Text Reader

Abstract

The present application relates to the technical field of electrical insulation materials, and specifically discloses a mica paper treatment liquid, mica paper, mica board, and its preparation method and application. The mica paper treatment liquid provided in the present application includes the following components in parts by weight: 20-40 parts of organic silica gel, 30-40 parts of aluminum nitride powder, 30-40 parts of wollastonite, and 0.3-2 parts of silane coupling agent; the thermal conductivity of the organic silica gel is 1.2-1.5W / (m·K); the present application also provides mica paper and mica board obtained by treatment with the above-mentioned mica paper treatment liquid; the mica board provided in the present application is formed by hot-pressing a plurality of mica papers, and the surfaces of both sides of the mica board are also coated with an insulating coating treatment liquid, wherein the temperature of the hot-pressing compound is 130-220°C, and the hot-pressing pressure is 2.0-2.6MPa. The mica board provided in the present application has excellent thermal insulation and high-temperature insulation properties, and can meet the use requirements of thermal runaway protection materials for power batteries of new energy vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrical insulation materials, and in particular to a mica paper treatment liquid, mica paper, a mica board, and a preparation method and application thereof. Background Art

[0002] With the continuous development of new energy vehicles, batteries, as the core components of new energy vehicles, play a major role in new energy vehicles. However, when new energy vehicles are subjected to external impact, excessive charging and discharging, heat accumulation, etc., it is easy to cause abnormal temperature rise of the battery, causing dangers such as fire or explosion, posing a potential threat to the safety of the vehicle and the driver and passengers.

[0003] At present, the thermal runaway protection materials for power batteries of new energy vehicles on the market are mainly mica boards, which are usually made by pressing and compounding multiple layers of mica paper with silicone resin, and their insulation performance mainly depends on the insulation performance of the mica paper itself. However, as the thermal runaway protection materials for power batteries of new energy vehicles have higher and higher requirements for thermal insulation and high-temperature insulation, the existing mica boards can no longer meet the use requirements of thermal runaway protection materials for power batteries of new energy vehicles. Therefore, it is urgent to improve the mica boards so that the mica boards can obtain higher thermal insulation and high-temperature insulation performance. Summary of the invention

[0004] In order to improve the thermal insulation and high-temperature insulation of mica boards, the present application provides a mica paper treatment liquid, mica paper, a mica board, and a preparation method and application thereof.

[0005] In a first aspect, the present application provides a mica paper treatment liquid, which adopts the following technical solution;

[0006] A mica paper treatment liquid comprises the following components in parts by weight: 20-40 parts of organic silica gel, 30-40 parts of aluminum nitride powder, 30-40 parts of wollastonite and 0.2-2 parts of a silane coupling agent;

[0007] The thermal conductivity of the organic silica gel is 1.2-1.5 W / (m·K).

[0008] The present application provides a mica paper treatment liquid, which is used to treat mica paper. The organic silica gel, aluminum nitride powder, wollastonite and other materials in the mica paper treatment liquid can penetrate well into the gaps in the mica paper scale structure, thereby improving the thermal insulation and high-temperature insulation performance of the mica paper. In the present application, the mica paper is made of crushed mica sheets, which are crushed into small flakes by a special process and then processed by a papermaking machine. Therefore, there are a large number of gaps inside the mica paper; the organic silica gel is a high-temperature resistant organic silica gel, which has excellent high-temperature resistance, insulation and adhesion; aluminum nitride powder is a ceramic material, which has good insulation, but aluminum nitride has a certain thermal conductivity, so its thermal insulation performance is poor, so the amount of aluminum nitride powder needs to be strictly controlled. Wollastonite is a single-chain silicate mineral, and its main component is Ca 3 Si 3 O 9 Wollastonite has good thermal insulation and flame retardancy, and can effectively prevent heat transfer. Silane coupling agent can increase the viscosity of mica paper treatment liquid, thereby increasing the bonding effect between mica papers.

[0009] In the present application, the addition amount of organic silica gel, aluminum nitride powder, wollastonite and silane coupling agent in the mica paper treating solution will affect the performance of the mica paper treating solution and the performance of the mica paper obtained. When the amount of organic silica gel added is greater than 45 parts, the uniformity of the mica paper treating liquid is poor, resulting in an uneven coating formed on the surface of the mica paper; when the amount of organic silica gel added is less than 20 parts, the mica paper treating liquid cannot be solidified because the amount of organic silica gel added is too small; when the amount of aluminum nitride powder added is greater than 40 parts, the coating formed on the surface of the mica paper by the mica paper treating liquid cracks, and the thermal insulation of the mica paper is poor; when the amount of aluminum nitride powder added is less than 30 parts, the insulation of the prepared mica paper is poor; when the amount of wollastonite added is greater than 40 parts, an insoluble white solid will appear in the mica paper treating liquid, and the coating formed on the surface of the mica paper by the mica paper treating liquid will fall off; when the amount of wollastonite added is less than 30 parts, the uniformity of the mica paper treating liquid is poor, resulting in an uneven coating formed on the surface of the mica paper. When the amount of silane coupling agent added is less than 0.3 parts, the mica paper treatment liquid is difficult to solidify due to the small amount of coupling agent added, the coating surface is sticky and easy to stick. Therefore, the application controls the amount of each component of the mica paper treatment liquid to be added within the above range, which can ensure the uniformity and stability of the mica paper treatment liquid, and the prepared mica paper has excellent heat insulation and high temperature insulation, and will not crack, powder, etc.

[0010] In a specific embodiment, the weight proportion of the organic silica gel may be 20 parts, 25 parts, 30 parts, 35 parts or 40 parts.

[0011] In a specific embodiment, the weight proportion of the aluminum nitride powder may also be: 30 parts, 33 parts, 35 parts, 38 parts or 40 parts.

[0012] In a specific embodiment, the weight proportion of the wollastonite may also be: 30 parts, 33 parts, 35 parts, 38 parts or 40 parts.

[0013] In a specific embodiment, the weight portion of the silane coupling agent can be: 0.3 parts, 1 part or 2 parts.

[0014] Preferably, the mica paper treating liquid comprises the following components in parts by weight: 25-35 parts of organic silica gel, 33-38 parts of aluminum nitride powder, 33-38 parts of wollastonite and 0.2-2 parts of silane coupling agent.

[0015] The present application further controls the weight of each component of the mica paper processing liquid within the above range, so that the obtained mica paper processing liquid has better uniformity and stability, and the obtained mica paper has better thermal insulation and high-temperature insulation properties.

[0016] A method for preparing a mica paper treating liquid comprises the following steps: stirring each component of the mica paper treating liquid at a rate of ≥300 r / min for ≥45 min to obtain the mica paper treating liquid.

[0017] In a second aspect, the present application provides a mica paper, which is obtained by treating with a mica paper treating liquid.

[0018] Preferably, the mica paper is double-sided coated with a mica paper treatment liquid; the thickness of the mica paper obtained after the double-sided coating is 0.2±0.05 mm.

[0019] In a second aspect, the present application provides a mica board, which includes the aforementioned mica paper processing liquid or mica paper.

[0020] Preferably, the mica board is formed by hot-pressing a plurality of mica papers; both side surfaces of the mica board are also coated with an insulating coating treatment liquid; the insulating coating treatment liquid comprises the following components in parts by weight: 15-25 parts of organic silica gel, 10-20 parts of fumed silica, 15-25 parts of aluminum nitride powder and 0.3-2 parts of silane coupling agent; the thermal conductivity of the organic silica gel is 1.2-1.5 W / (m·K).

[0021] In the present application, by compounding and extruding multiple mica papers into a mica board, and then coating a layer of insulating coating treatment liquid on the surface of the mica board, a vitrified insulating coating can be formed on the surface of the mica board, so that the mica board has excellent thermal insulation and high-temperature insulation properties. In the insulating coating treatment liquid, when the addition amount of organic silica gel is less than 15 parts, the obtained insulating coating treatment liquid cannot be cured on the surface of the mica board and it is difficult to form a porcelain coating; when the addition amount of organic silica gel is greater than 20 parts, the insulating coating treatment liquid cracks after curing on the surface of the mica board, and the thermal insulation and high-temperature insulation of the mica board are poor; when the addition amount of fumed silica is less than 10 parts, the insulation of the prepared mica board is poor; when the addition amount of fumed silica is greater than 20 parts, the insulating coating treatment liquid contains white flocs; when the addition amount of aluminum nitride powder is less than 15 parts, the coating formed on the surface of mica paper by the insulating coating treatment liquid is easy to fall off at high temperature; when the addition amount of aluminum nitride powder is greater than 25 parts, the coating formed on the surface of mica paper by the insulating coating treatment liquid will show powdering phenomenon. Therefore, the present application controls the addition amount of each component of the insulating coating treatment liquid within the above-mentioned range, and can obtain an insulating coating treatment liquid with good uniformity and excellent insulating performance. By coating the surface of the mica board with the insulating coating treatment liquid, the thermal insulation and high-temperature insulation performance of the mica board can be improved, and the ceramic coating on its surface performance is smooth and firm.

[0022] In the present application, the fumed silica has excellent insulation properties. Compared with conventional silica, its particles are smaller, and its thickening and distribution uniformity are better, so the insulation effect of the obtained mica board is also better.

[0023] In a specific embodiment, the weight proportion of the organic silica gel may be 15 parts, 20 parts or 25 parts.

[0024] In a specific embodiment, the weight proportion of the fumed silica may also be 10 parts, 15 parts or 20 parts.

[0025] In a specific embodiment, the weight proportion of the aluminum nitride powder may also be 15 parts, 20 parts or 25 parts.

[0026] In a specific embodiment, the weight portion of the silane coupling agent may be: 1 part.

[0027] Preferably, the thickness of the coating formed by the insulating coating treatment liquid on both sides of the mica board is 0.15-0.25 mm.

[0028] Preferably, the mica board has a thickness of 1.8-2.5 mm, a normal withstand voltage of 60 kv / mm, and a 1000°C withstand voltage of 30 kv / mm.

[0029] A method for preparing a thermal insulation coating treatment liquid comprises the following steps: stirring the components of the thermal insulation coating treatment liquid at a rate of ≥300 r / min for ≥45 min to obtain the thermal insulation coating treatment liquid.

[0030] In a third aspect, the present application provides a method for preparing a mica board.

[0031] A method for preparing a mica plate comprises the following steps:

[0032] (1) firstly, the mica paper is soaked with a mica paper treatment liquid or the mica paper is double-sided coated so that a coating with a thickness of 0.2±0.05 mm is formed on both sides of the mica paper;

[0033] (2) compounding a plurality of mica papers obtained in step (1), and then hot pressing at 130-220° C. and 2.0-2.6 MPa for 15-30 min to obtain a prefabricated mica board;

[0034] (3) Then, the insulating coating treatment liquid is coated on both sides of the mica board obtained in step (2), and the mica board is obtained by two-stage drying; in the two-stage drying, the first stage is dried at a temperature of 80±10°C and the time is 5-10min; the second stage is dried at a temperature of 100±10°C and the time is 10-20min.

[0035] The present application provides a method for preparing a mica board, which first uses a mica paper treatment liquid to treat the mica paper, then performs composite extrusion on the treated mica paper to obtain a mica board, and finally obtains a mica board by applying an insulating coating treatment liquid to the surface of the mica board. The present application experimentally explored and found that in the preparation steps of the mica board: when the temperature of the hot press is lower than 130°C, the adhesion between the mica papers is poor, and the mica board is prone to delamination; when the temperature of the hot press is higher than 220°C, bubbles will appear in the thermal insulation glue layer (formed by the curing of the insulating coating treatment liquid) on the surface of the mica board; when the pressure of the hot press is less than 2.0MPa, the adhesion between the mica papers is poor, and the mica board is prone to delamination; when the pressure of the hot press is greater than 2.6MPa, the thermal insulation glue layer on the surface of the mica board is squeezed and thinned, and the thermal insulation of the mica board is poor. Therefore, the present application controls the extrusion temperature and pressure within the above range, and can obtain a mica board with good bonding properties and excellent insulation and heat insulation properties. The mica board can fully meet the use requirements of thermal runaway protection materials for new energy vehicle power batteries.

[0036] In the present application, when the first stage drying temperature is lower than 70°C and the second stage drying temperature is lower than 90°C, the insulating coating treatment liquid on the surface of the mica board cannot be cured, and the surface of the mica board becomes sticky; when the first stage drying temperature is higher than 90°C and the second stage drying temperature is higher than 120°C, the insulating coating treatment liquid on the surface of the mica board will produce bubbles during the curing process, and the formed thermal insulation adhesive layer contains micropores, and the thermal insulation and high-temperature insulation of the mica board are relatively low. Therefore, the present application controls the parameters of the two-stage drying within the above range, which can ensure that the insulating coating treatment liquid on the surface of the mica board can be smoothly cured into a dense, dry, vitrified coating, thereby obtaining a mica board with excellent insulation and heat insulation properties.

[0037] In a fourth aspect, the present application provides mica paper treatment liquid, mica paper and mica board for use in power batteries for new energy vehicles.

[0038] In summary, this application has the following beneficial effects:

[0039] 1. The present application adopts a specific ratio of organic silica gel, aluminum nitride powder, wollastonite and silane coupling agent to prepare a mica paper processing liquid, and uses the mica paper processing liquid to dip or double-sided coat the mica paper. The inorganic material in the mica paper processing liquid can well enter the gaps in the mica paper flake structure, thereby improving the thermal insulation and high-temperature insulation properties of the mica paper.

[0040] 2. The present application uses mica paper treatment liquid dipped in glue or double-sided coated mica paper to form a mica board by hot pressing. By controlling the hot pressing pressure and temperature, the bonding performance, thermal insulation performance, and insulation performance of the mica board can be made more excellent, and it is ensured that the mica board after hot pressing does not delaminate and has no glue overflow. Then, an insulating coating treatment liquid is applied to the surface of the mica board. After curing, the insulating coating treatment liquid will form a vitrified coating on the surface of the mica board, further improving the fireproof, flame retardant, and high-temperature insulation performance of the outer surface of the mica board.

[0041] 3. The insulating coating treatment liquid of the present application is made of 15-25 parts of organic silica gel, 10-20 parts of fumed silica, 15-25 parts of aluminum nitride powder and a silane coupling agent. The insulating coating treatment liquid with the above proportion can form a dense ceramic coating on the surface of the mica board, which has excellent fire prevention, heat insulation and insulation effects.

[0042] 4. The thickness of the mica board obtained in this application is 1.8-2.5mm, the normal withstand voltage is 60kv / mm, the withstand voltage at 1000℃ is 30kv / mm, and after one side of the mica board is burned at 1000℃ for 10 minutes, the temperature of the other side is only 150℃. The mica board has excellent thermal insulation and high-temperature insulation properties, and can fully meet the use requirements of thermal runaway protection materials for new energy vehicle power batteries. DETAILED DESCRIPTION

[0043] In a first aspect, the present application provides a mica paper treatment liquid, which includes the following components in parts by weight: 20-40 parts of organic silica gel, 30-40 parts of aluminum nitride powder, 30-40 parts of wollastonite, and 0.3-2 parts of a silane coupling agent; the thermal conductivity of the organic silica gel is 1.2-1.5 W / (m·K). Further, the mica paper treatment liquid includes the following components in parts by weight: 25-35 parts of organic silica gel, 33-38 parts of aluminum nitride powder, 33-38 parts of wollastonite, and 0.2-2 parts of a silane coupling agent.

[0044] The preparation method of the mica paper treating liquid is as follows: stirring the components of the mica paper treating liquid at a rate of ≥300 r / min for ≥45 min to obtain the mica paper treating liquid.

[0045] In a second aspect, the present application provides a mica paper obtained by double-sided coating with a mica paper treatment liquid; the coating thickness formed on the surface of the mica paper by the mica paper treatment liquid is 0.2±0.05 mm.

[0046] In the third aspect, the present application provides a mica board, which is formed by hot pressing a plurality of mica papers; the hot pressing temperature is 130-220°C, and the hot pressing pressure is 2.0-2.6MPa. Furthermore, both sides of the mica board are coated with an insulating coating treatment liquid; the insulating coating treatment liquid includes the following components in parts by weight: 15-25 parts of organic silica gel, 10-20 parts of fumed silica, 15-25 parts of aluminum nitride powder, and 0.3-2 parts of silane coupling agent; the thermal conductivity of the organic silica gel is 1.2-1.5W / (m·K).

[0047] The preparation method of the above-mentioned thermal insulation coating treatment liquid is: stirring the components of the thermal insulation coating treatment liquid at a rate of ≥300r / min for ≥45min to obtain the thermal insulation coating treatment liquid.

[0048] The method for preparing the mica plate comprises the following steps:

[0049] (1) firstly, the mica paper is soaked with a mica paper treatment liquid or the mica paper is double-sided coated so that a coating with a thickness of 0.2±0.05 mm is formed on both sides of the mica paper;

[0050] (2) compounding a plurality of mica papers obtained in step (1), and then hot pressing at 130-220° C. and 2.0-2.6 MPa for 15-30 min to obtain a prefabricated mica board;

[0051] (3) Then, the insulating coating treatment liquid is applied to both sides of the mica board obtained in step (2), and the mica board is obtained by two-stage drying. In the two-stage drying, the first stage is dried at a temperature of 80±10°C for 5-10 minutes, and the second stage is dried at a temperature of 100±10°C for 10-20 minutes.

[0052] In the embodiments of the present application, organic silica gel was purchased from Hubei Xinsihai Chemical Co., Ltd.; aluminum nitride powder was purchased from Shanghai Xiaohuang Nano Technology Co., Ltd.; wollastonite was 800 mesh, purchased from Jiangxi Aote Technology Co., Ltd.; silane coupling agent was KH550, purchased from Nanjing Pinning Coupling Agent Co., Ltd.; the model of fumed silica was HB151, purchased from Hubei Huifu Nanomaterial Co., Ltd.; the model of aluminum nitride powder was AIN-H, purchased from Liaoning Desheng Special Ceramics Manufacturing Co., Ltd.; the model of mica paper was P506, purchased from Pingjiang County Weipai Mica Insulation Material Co., Ltd.; the remaining raw materials, reagents, solvents, etc. can also be obtained commercially.

[0053] The present application is further described in detail below in combination with preparation examples, embodiments and performance testing experiments.

[0054] Preparation Example 1-15

[0055] Preparation Examples 1-15 respectively provide a mica paper processing liquid. The difference between the above mica paper processing liquids lies in: the amount of each component of the mica paper processing liquid; the specific details are shown in Table 1 below.

[0056] The preparation method of the mica paper treatment liquid provided in Preparation Example 1-15 is: weigh the components according to the addition amount in Table 1, mix them, and stir them at a speed of 400 r / min for 45 minutes to obtain the mica paper treatment liquid.

[0057] Table 1 Components and addition amounts of mica paper treatment solutions provided in Preparation Examples 1-15

[0058]

[0059]

[0060] Comparative Preparation Examples 1-7

[0061] Comparative Preparation Examples 1-7 were prepared according to the preparation method of Preparation Example 3, except that: the amount of each component of the mica paper treatment solution was as shown in Table 2 below.

[0062] Table 2 Comparative Preparation Examples 1-7 provided by the composition and addition amount of mica paper treatment solution

[0063]

[0064] Comparative Preparation Example 8

[0065] Comparative Preparation Example 8 was prepared according to the preparation method of Preparation Example 3, except that the components and amounts of the mica paper treatment liquid were: 30 g of organic silica gel, 35 g of aluminum nitride powder, 35 g of nano aerogel, and 1 g of silane coupling agent.

[0066] Comparative Preparation Example 9

[0067] Comparative Preparation Example 9 was prepared according to the preparation method of Preparation Example 3, except that the components and amounts of the mica paper treatment liquid were: 50 g of organic silica gel, 10 g of aluminum nitride powder, and 20 g of nano aerogel.

[0068] Comparative Preparation Example 10

[0069] Comparative Preparation Example 10 was carried out according to the preparation method of Preparation Example 3, except that: the components and amounts of the mica paper treatment liquid were: 30 g of polyimide resin solution, 35 g of aluminum nitride powder, 35 g of wollastonite, and 1 g of silane coupling agent.

[0070] Preparation Examples 16-22

[0071] Preparation Examples 16-22 provide an insulating coating treatment solution. The difference between the above insulating coating treatment solutions is that the amount of each component of the insulating coating treatment solution is as shown in Table 3 below.

[0072] The preparation method of the insulating coating treatment liquid provided in Preparation Examples 16-22 is: weigh and mix the components according to the addition amounts in Table 3, stir the components of the insulating coating treatment liquid at a rate of 400 r / min for 45 minutes to obtain the insulating coating treatment liquid.

[0073] Table 3 Components and addition amounts of the insulating coating treatment solution provided in Preparation Examples 16-22

[0074]

[0075]

[0076] Comparative Preparation Examples 11-16

[0077] Comparative Preparation Examples 11-16 were prepared according to the method of Preparation Example 17, except that the amounts of the components of the insulating coating treatment solution were as shown in Table 4 below.

[0078] Table 4 Comparative composition and addition amount of the insulating coating treatment solution provided by Preparation Examples 11-16

[0079]

[0080] Comparative Preparation Example 17

[0081] Comparative Preparation Example 17 was carried out according to the method of Preparation Example 17, except that the fumed silica was replaced by ordinary silica.

[0082] Examples 1-15

[0083] Examples 1-15 provide a mica board respectively, and the difference between the above mica boards is that the mica paper processing liquid in the mica board is derived from Preparation Examples 1-15 respectively.

[0084] The preparation method of the mica plate is as follows:

[0085] (1) firstly, the mica paper is soaked with a mica paper treatment liquid or the mica paper is double-sided coated so that a coating with a thickness of 0.2±0.05 mm is formed on both sides of the mica paper;

[0086] (2) compounding a plurality of mica papers obtained in step (1), and then hot pressing at 180° C. and 2.4 MPa for 20 min to obtain a prefabricated mica board;

[0087] (3) Then, the insulating coating treatment liquid (Preparation Example 17) is coated on both sides of the mica board obtained in step (2), and the mica board is obtained by two-stage drying; in the two-stage drying, the first stage is dried at a temperature of 80°C and the time is 5 minutes; the second stage is dried at a temperature of 100°C and the time is 10 minutes.

[0088] Comparative Examples 1-10

[0089] Comparative Examples 1-10 each provide a mica board.

[0090] Comparative Examples 1-10 were prepared according to the method of Example 3, except that the mica paper treatment liquid in the mica boards of Comparative Examples 1-10 was derived from Comparative Preparation Examples 1-10, respectively.

[0091] Examples 16-21

[0092] Embodiments 16-21 each provide a mica board.

[0093] Examples 16-21 were carried out according to the method of Example 3, except that the sources of the insulating coating treatment liquid in Examples 16-21 were specifically shown in Table 5.

[0094] Table 5 Sources of the insulating coating treatment liquid in the mica board provided by Examples 16-21

[0095] / Sources of Insulation Coating Treatment Fluids / Sources of Insulation Coating Treatment Fluids Example 3 Preparation Example 17 Embodiment 19 Preparation Example 20 Example 16 Preparation Example 16 Embodiment 20 Preparation Example 21 Embodiment 17 Preparation Example 18 Embodiment 21 Preparation Example 22 Embodiment 18 Preparation Example 19

[0096] Comparative Examples 11-17

[0097] Comparative Examples 11-17 each provide a mica board.

[0098] Comparative Examples 11-17 were prepared according to the method of Example 3, except that the insulating coating treatment liquids in the mica boards of Comparative Examples 11-17 were derived from Comparative Preparation Examples 11-17, respectively.

[0099] Examples 22-28

[0100] Embodiments 22-28 each provide a mica board.

[0101] Examples 22-28 were carried out according to the method of Example 3, except that some parameters in the mica board preparation method are specifically shown in Table 6.

[0102] Table 6 Partial parameters of the preparation method of mica board provided in Examples 22-28

[0103]

[0104]

[0105] Comparative Example 18

[0106] Comparative Example 18 provides a mica board.

[0107] Comparative Example 18 was carried out according to the method of Example 3, except that: in the preparation method of the mica board provided in Comparative Example 18, the hot pressing temperature was 250°C.

[0108] Comparative Example 19

[0109] Comparative Example 19 provides a mica board.

[0110] Comparative Example 19 was carried out according to the method of Example 3, except that: in the preparation method of the mica board provided in Comparative Example 19, the hot pressing pressure was 2.8 MPa.

[0111] Comparative Example 20

[0112] Comparative Example 20 provides a mica board.

[0113] Comparative Example 20 was carried out according to the method of Example 3, except that: step (3) of the mica board preparation method is as follows:

[0114] (3) Then, the insulating coating treatment liquid is applied to both sides of the mica board obtained in step (2), and then dried at 100°C for 10 minutes to obtain a mica board. (With bubbles)

[0115] The performance testing test was carried out on the physical properties and performance of the mica boards obtained in Examples 1-29 and Comparative Examples 1-20 of the present application. The results are shown in Table 7.

[0116] (1) Physical properties: including whether the surface of mica paper and mica board is flat at room temperature, whether there are bubbles, whether there is white powder, and whether there are cracks. Note: When the surface properties of mica paper or mica board are not good, the thermal insulation and voltage resistance related performance tests are abandoned, which is indicated by " / " in Table 7.

[0117] (2) Thermal insulation: Burn one side of the mica board in a 1000°C flame for 10 minutes, and then measure the temperature of the other side of the mica board.

[0118] (3) Normal withstand voltage: Use a withstand voltage tester to perform a pressure test on the mica board under normal conditions. For specific methods, please refer to GB / T5019.2-2009 "Mica-based insulating materials" Part 2: Test methods.

[0119] (4) High temperature withstand voltage: Use a withstand voltage tester to perform a pressure test on the mica board at 1000°C. For specific methods, please refer to GB / T5019.2-2009 "Mica-based insulating materials" Part 2: Test methods.

[0120] Table 7 Performance test results of mica boards of Examples 1-29 and Comparative Examples 1-20

[0121]

[0122]

[0123]

[0124]

[0125] According to the test results in Table 7, the mica board provided in Examples 1-29 of the present application has a flat surface, no bubbles, no powder, and no cracks. One side of the mica board is burned at 1000°C for 10 minutes, and the surface temperature of the other side is ≤150°C, indicating that the mica board has excellent thermal insulation performance; and the withstand voltage of the above mica board under normal conditions is 57-66kv / mm, and the withstand voltage at a high temperature of 1000°C is 30-37kv / mm, indicating that the above mica board has excellent insulation performance. Therefore, the mica board provided in the present application has excellent thermal insulation and high-temperature insulation performance, and can fully meet the use requirements of thermal insulation materials for new energy vehicles.

[0126] In Comparative Example 1, since the content of the organic silicone resin in the mica paper treating liquid is relatively low, the mica paper treating liquid cannot be cured and it is difficult to form a coating on the surface of the mica paper.

[0127] In Comparative Example 2, due to the high content of silicone resin in the mica paper treating liquid, the viscosity of the mica paper treating liquid is relatively high, and the uniformity of the coating formed on the surface of the mica paper is relatively poor; the thermal insulation and electrical insulation properties of the mica board made using the mica paper are relatively low.

[0128] Although the mica board obtained in Comparative Example 3 has a smooth surface, no bubbles, no powder, and no cracks, the insulation of the mica board is poor due to the low content of aluminum nitride powder in the mica paper processing liquid.

[0129] In Comparative Example 4, due to the high content of aluminum nitride powder in the mica paper treatment solution, the coating on the surface of the mica paper cracked.

[0130] In Comparative Example 5, due to the low content of wollastonite in the mica paper treating solution, the viscosity of the mica paper treating solution is relatively high, and the uniformity of the coating formed on the surface of the mica paper is relatively poor; the thermal insulation and electrical insulation properties of the mica board made of the mica paper are relatively low.

[0131] In Comparative Example 6, due to the high content of wollastonite in the mica paper treating solution, after the mica paper treating solution solidifies on the surface of the mica paper, white powder appears on the surface of the mica paper, and powder falling occurs.

[0132] In Comparative Example 7, due to the low content of the silane coupling agent, the mica paper treating liquid is still sticky after the mica paper treating liquid is solidified on the surface of the mica paper.

[0133] Although the mica boards obtained in Comparative Examples 8-10 have a smooth surface, no bubbles, no powder, and no cracks, their heat insulation and electrical insulation properties are relatively low.

[0134] In Comparative Example 11, due to the low content of organic silicone resin in the insulating coating treatment liquid, the insulating coating treatment liquid cannot be cured on the surface of the mica board, and it is difficult to form a vitrified coating.

[0135] In Comparative Example 12, due to the high content of silicone resin in the insulating coating treatment liquid, the viscosity of the insulating coating treatment liquid is relatively high, the ceramic coating formed on the surface of the mica board cracks, and the thermal insulation and electrical insulation properties of the mica board are relatively low.

[0136] Although the mica board obtained in Comparative Example 13 has a smooth surface, no bubbles, no powder, and no cracks, the insulation of the mica board is poor due to the low content of aluminum nitride powder in the insulating coating treatment liquid.

[0137] In Comparative Example 14, since the aluminum nitride powder content in the insulating coating treatment liquid is relatively high, after the insulating coating treatment liquid is solidified on the surface of the mica board, white powder appears on the surface of the mica board, and powder falling occurs.

[0138] The ceramic coating on the surface of the mica plate obtained in Comparative Example 15 fell off at 1000°C.

[0139] The mica board obtained in Comparative Example 16 had white powder on its surface and powder falling occurred.

[0140] In Comparative Example 17, the ceramic coating on the surface of the mica board obtained by using conventional silica has obvious particulate impurities, poor coating uniformity, and slightly low insulation performance.

[0141] In Comparative Example 18, due to the excessively high hot pressing temperature, bubbles appeared in the insulating coating treatment liquid on the surface of the mica board during the hot pressing process, and the density of the formed ceramic coating was poor, and the insulation and heat insulation properties of the mica board finally obtained were low.

[0142] In Comparative Example 19, due to excessive hot pressing pressure, the coatings in the mica board were squeezed and thinned, which resulted in low insulation and heat insulation properties of the mica board.

[0143] When comparative example 20 only adopts one-stage drying, bubbles appear in the insulating coating treatment liquid on the surface of the mica board during the hot pressing process, the density of the formed ceramic coating is poor, and the insulation and heat insulation properties of the mica board finally obtained are low.

[0144] In summary, the mica board provided in the present application has excellent thermal insulation and high-temperature insulation properties, and can fully meet the thermal insulation and high-temperature insulation requirements of thermal runaway protection materials for power batteries of new energy vehicles.

[0145] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A mica board, characterized in that: The mica board is formed by hot-pressing a plurality of mica papers; both sides of the mica board are also coated with an insulating coating treatment liquid; the insulating coating treatment liquid is made of the following components in parts by weight: 15-25 parts of organic silica gel, 10-20 parts of fumed silica, 15-25 parts of aluminum nitride powder and 0.3-2 parts of a silane coupling agent; The mica paper is coated on both sides with a mica paper treatment liquid, wherein the mica paper treatment liquid is made of the following components in parts by weight: 20-40 parts of organic silica gel, 30-40 parts of aluminum nitride powder, 30-40 parts of wollastonite and 0.3-2 parts of a silane coupling agent; The thermal conductivity of the organic silica gel is 1.2-1.5 W / (m·K); The normal withstand voltage of the mica board is 60kv / mm; the withstand voltage at 1000°C is 30kv / mm.

2. The mica board according to claim 1, characterized in that: The mica paper treatment liquid is made of the following components in parts by weight: 25-35 parts of organic silica gel, 33-38 parts of aluminum nitride powder, 33-38 parts of wollastonite and 0.2-2 parts of silane coupling agent.

3. The mica board according to claim 1, characterized in that: The coating thickness formed by the mica paper treating liquid on the surfaces of both sides of the mica paper is 0.2±0.05 mm.

4. The mica board according to claim 1, characterized in that: The thickness of the coating formed by the insulating coating treatment liquid on both sides of the mica board is 0.15-0.25mm.

5. The mica board according to claim 1, characterized in that: The thickness of the mica plate is 1.8-2.5 mm.

6. The method for preparing a mica board according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) First, the mica paper is double-sided coated with a mica paper treatment liquid so that a coating with a thickness of 0.2±0.05 mm is formed on both sides of the mica paper; (2) Compounding the mica papers obtained in the multiple steps (1), and then hot pressing for 15-30 min at 130-220° C. and 2.0-2.6 MPa to obtain a prefabricated mica board; (3) Then, the insulating coating treatment liquid is coated on both sides of the prefabricated mica board obtained in step (2), and the mica board is obtained by two-stage drying; in the two-stage drying, the first stage is dried at a temperature of 80±10°C and the time is 5-10 minutes; the second stage is dried at a temperature of 100±10°C and the time is 10-20 minutes.

7. Application of the mica board as described in any one of claims 1 to 5 in a power battery for new energy vehicles.