A method for preparing nickel ferrite-based eutectic ceramic inert anode material
Through eutectic ceramic preparation technology, the density and performance of nickel-ferrate-based ceramic materials are improved, the corrosion problem of ceramic anode materials in the electrolytic aluminum process is solved, the process flow is simplified, and the performance and process improvement is achieved.
Patent Information
- Application Number
- CN202311818746.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-27
AI Technical Summary
The existing nickel-ferrate-based ceramic inert anode materials have priority corrosion in the grain boundary during the electrolytic aluminum process, resulting in micropores on the surface, reducing their corrosion resistance and electrical conductivity. The traditional firing process is complex and it is difficult to achieve industrial manufacturing.
Using eutectic ceramic preparation technology, NiFe2O4-based spinel powder is mixed with nickel-chlorite powder, added binder and pressed into molding, prefixed, melted, cooled and solidified in an inert atmosphere, followed by heat treatment, and adjusting the microstructure structure. Improve material density and performance.
It significantly improves the density, conductivity and corrosion resistance of the material, simplifies the preparation process, reduces grain boundary defects in the sintering process of traditional ceramics, and realizes the improvement of the performance of ceramic anode materials and the transformation of process.
Abstract
Description
Technical Field
[0001] The invention relates to aluminum electrolytic processing related technologies, and in particular to a method for preparing a nickel ferrite-based eutectic ceramic inert anode material. Background Art
[0002] Nickel ferrite ceramics have become a hot ceramic material in the electrolytic aluminum industry in recent decades due to their good electrical conductivity and certain resistance to high-temperature molten salt corrosion. The main reason is that this type of ceramic inert anode can reduce carbon emissions during the electrolytic aluminum electrolysis process.
[0003] In order to achieve a balance between density, mechanical properties, conductivity and resistance to high-temperature molten salt corrosion, nickel ferrite-based ceramic inert anodes often add different oxide components to improve conductivity, thermal shock resistance and corrosion resistance, forming a large class of ceramic anode materials.
[0004] Tests and studies under actual production conditions have shown, through high-temperature molten salt corrosion experiments, that this type of ceramic inert anode corrodes preferentially at the grain boundaries during electrolysis, causing micropores to appear on the surface of the ceramic inert anode, providing a penetration channel for the high-temperature molten salt electrolyte, and the ceramic inert anode is further electrochemically and chemically corroded.
[0005] In order to improve the corrosion resistance, thermal shock resistance and electrical conductivity of ceramic anodes, the existing technology has proposed many methods and measures to improve the density of ceramic sintering, but the effect of improving the corrosion resistance, thermal shock resistance and electrical conductivity of ceramic materials is not great. In addition, according to the traditional ceramic production process, it is very difficult to fire large ceramic anodes. The industrialization of such ceramic anodes is extremely difficult, and the related molding and firing process technologies are complex. The technical problems faced by ceramic anodes in the process of industrialization of electrolytic aluminum reduction are still very prominent. Summary of the invention
[0006] In view of the defects or shortcomings of the prior art, the present invention provides a method for preparing a nickel ferrite-based eutectic ceramic inert anode material.
[0007] To this end, the preparation method of the nickel ferrite-based eutectic ceramic inert anode material provided by the present invention comprises:
[0008] Step 1, preparing a pre-sintered body:
[0009] The mixed powder of NiFe2O4-based spinel powder and nickel green stone powder is mixed with a binder and granulated into 10-30 mesh granules; the granules are then pressed under a pressure of 100-200 MPa to obtain a green body; and the green body is pre-sintered for 2-5 hours at 1100-1300° C. in an inert gas atmosphere to obtain a pre-sintered body;
[0010] Calculated as 100% by mass, the mass percentage of the NiFe2O4-based spinel is 80wt% to 90wt%, and the mass percentage of the nickel green stone is 10wt% to 20wt%; the binder is selected from one or a mixture of two or more of polyvinyl alcohol and polyethylene glycol, and the mass of the binder accounts for 0.5wt% to 2wt% of the mass of the mixed powder;
[0011] Step 2: Pre-sintered body melting and cooling solidification:
[0012] The pre-sintered body is heated and melted in an inert gas atmosphere to make the pre-sintered body molten; then the molten material is cooled and solidified at a cooling rate of 1-100°C / min, or the molten material is cast and then cooled and solidified at a cooling rate of 1-100°C / min to obtain a ceramic solidified body;
[0013] Step 3, heat treatment:
[0014] The ceramic solid body obtained in step 2 is treated at a temperature of 1250-1400°C for 2-6 hours to adjust the microstructure and eliminate stress; then cooled to room temperature at a cooling rate of 1-50°C / min to obtain a nickel ferrite-based eutectic ceramic inert anode material.
[0015] An optional solution is that the NiFe2O4-based spinel composition is: NiFe2O4 accounts for 20wt% to 80wt%; ZnFe2O4 accounts for 0wt% to 20wt%; CuFe2O4 accounts for 0wt% to 20wt%; CoFe2O4 accounts for 0wt% to 20wt%; MnFe2O4 accounts for 0wt% to 20wt%; and does not include the endpoint value 0.
[0016] An optional solution is that the nickel green stone composition is: NiO accounts for 20wt% to 80wt%; CaO accounts for 0wt% to 20wt%; CeO2 accounts for 0wt% to 20wt%; ZrO2 accounts for 0wt% to 20wt%; Al2O3 accounts for 0wt% to 20wt%; V2O5 accounts for 0wt% to 20wt%; and does not include the endpoint value 0.
[0017] Alternatively, the nickel chlorite is replaced by NiO.
[0018] Preferably, the particle size of the mixed powder is less than 100 mesh.
[0019] An optional solution is to ball-mill a mixture of NiFe2O4-based spinel powder, nickel green stone powder, dispersant and water for 12-24 hours to obtain a ceramic slurry; then dry and grind the ceramic slurry to obtain a mixed powder;
[0020] The dispersant is selected from one or a mixture of two or more of ethanol, ethylene glycol and glycerol, and the mass of the dispersant accounts for 1wt%-5wt% of the total mass of the NiFe2O4-based spinel powder and the nickel green stone powder;
[0021] The mass of the water is 3-5 times the total mass of the NiFe2O4-based spinel powder and the nickel green stone powder.
[0022] Alternatively, in step 2, the pre-sintered body is melted in an inert gas atmosphere at a temperature of 1650-1850° C. for 1-2 hours to make the pre-sintered body molten.
[0023] An optional solution is that the melting in step 2 is carried out by any one or a combination of arc melting, discharge plasma melting, laser suspension zone melting, optical floating zone melting, electron beam zone melting, high-frequency electromagnetic induction zone melting and energized Joule heat melting.
[0024] Furthermore, the nickel ferrite-based eutectic ceramic inert anode material prepared by the present invention has a density of 99%-100%, a thermal shock resistance of 95%-120%, a mechanical property of 70-110MPa, a high temperature corrosion resistance of 5-50 microns, and a conductivity of 8-30S / cm.
[0025] The present invention utilizes eutectic ceramic preparation technology to obtain dense nickel ferrite-based eutectic ceramic materials, which greatly reduces the corrosion of traditional ceramic grain boundaries. By increasing the density of the material, the electrical conductivity, mechanical properties and corrosion resistance of the material are improved. At the same time, through ceramic melting and casting, the traditional ceramic preparation process is simplified, thereby achieving a generational improvement in the performance of ceramic anode materials and a change in the preparation process.
[0026] The present invention greatly improves the density of nickel ferrite-based ceramic materials, eliminates grain boundary defects existing in the traditional sintering process of ceramics, and improves the overall performance of ceramic materials, including corrosion resistance, electrical conductivity, mechanical properties, etc. The preparation process of the present invention is easy to form, the process flow is simple, it is conducive to the control of ceramic shape and size, and it is easy to industrialize and engineer. DETAILED DESCRIPTION
[0027] Unless otherwise specified, the scientific and technical terms used herein are understood according to the knowledge of ordinary technicians in the relevant fields.
[0028] The present invention pre-sinters the nickel ferrite-based eutectic ceramic inert anode material, directly melts it at high temperature (the melting temperature can be determined according to the composition and properties of the material, so that the pre-sintered body can be heated and melted within a reasonable time), and then cools and solidifies, or cools and solidifies after casting. In a specific scheme, the nickel ferrite-based eutectic ceramic with excellent performance can be obtained by controlling the ceramic chemical composition, melting temperature and melting atmosphere, as well as the cooling rate and post-solidification heat treatment.
[0029] It should be noted that the temperature and amount of material used herein are approximate values for illustration purposes. Although methods and materials similar to or equivalent to the methods and materials described in the present invention can be used for the implementation of the present disclosure, some suitable methods and raw materials are described below. In addition, the raw materials, amounts and embodiments are only exemplary and are not intended to be limiting. In the specific scheme, those skilled in the art can optimize the raw materials, amount of material, and operating parameters involved in the method according to the disclosure of the present invention using conventional experimental time periods to achieve the purpose of the present invention.
[0030] The raw materials used in the following examples are all commercially available products, and the components of the materials are of analytical grade.
[0031] The composition of the NiFe2O4-based spinel used in the following examples is: NiFe2O4 accounts for 79.6wt%; ZnFe2O4 accounts for 5.8%; CuFe2O4 accounts for 2.6wt%; CoFe2O4 accounts for 0.9wt%; MnFe2O4 accounts for 10.4wt%;
[0032] The composition of the nickel green stone used is: NiO accounts for 78.3wt%; CaO accounts for 11.5wt%; CeO2 accounts for 0.8wt%; ZrO2 accounts for 1.1wt%; Al2O3 accounts for 6.7%; V2O5 accounts for 1.4wt%.
[0033] The performance testing methods of the materials described in this article are:
[0034] Density: Measured by Archimedes drainage method, it is the ratio of actual density to theoretical density.
[0035] Thermal shock resistance: The material is placed in a 960℃ high-temperature furnace from room temperature for 10 minutes and then taken out and cooled to room temperature in the air, completing a thermal shock. Then the material after the thermal shock is subjected to a bending strength test. The ratio of the strength after the thermal shock to that before the thermal shock is the strength residual rate (representing thermal shock resistance). The larger the strength residual rate, the better the thermal shock resistance of the material.
[0036] Mechanical properties: Mechanical properties are expressed by flexural strength, and flexural strength testing refers to GB / T4741-1999.
[0037] High temperature corrosion resistance: The NiFe2O4 eutectic ceramic inert anode material sintered at different temperatures was subjected to a high temperature molten salt static corrosion experiment. The inert anode material was placed in a high-purity graphite crucible filled with sufficient electrolyte, and the electrolyte composition was 90% industrial cryolite (molecular ratio of 2.2), 5% CaF2 and 5% Al2O3 (mass ratio); after being etched at 960°C for 8 hours, it was taken out and allowed to cool; the etched inert anode material was heated in a water bath with a mass percentage concentration of 30% AlCl3 solution to dissolve and fall off the residue on the surface of the material, and then the surface of the material was rinsed with clean water; the surface of the etched material was subjected to SEM and EDS elemental analysis. The thickness of the corrosion layer of the material was measured under a microscope, which represents the high temperature corrosion resistance of the material.
[0038] Conductivity: At 960°C, the current passing through the sample per unit area and per unit length is measured at a constant voltage, and the conductivity of the sample is calculated based on Ohm's law.
[0039] Based on the above detection method, the density of the material prepared by the present invention is 99%-100%; the thermal shock resistance is 95%-120%; the mechanical property is 70-110MPa; the high temperature corrosion resistance is 5-50 microns; and the electrical conductivity is 8-30S / cm.
[0040] Embodiment 1:
[0041] 1) Preparing a pre-sintered body: ball-milling a mixture of 85wt% NiFe2O4-based spinel powder, 15wt% nigericin powder, ethanol (accounting for 5wt% of the total mass of NiFe2O4-based spinel powder and nigericin powder) and water (4 times the total mass of NiFe2O4-based spinel powder and nigericin powder) for 14 hours to obtain a ceramic slurry with a particle size of less than 200 mesh; drying the ceramic slurry at 150±10°C and grinding it to obtain a mixed powder of less than 100 mesh, adding 1.5wt% of polyvinyl alcohol as a binder, and then granulating it into 10-30 mesh granules, and pressing the granules under a pressure of 150MPa to obtain a green body; then pre-calcining it at 1200±100°C in a nitrogen protective atmosphere for 4 hours to obtain a pre-sintered body;
[0042] 2) Melting and cooling of the pre-sintered body: The pre-sintered body is melted in a spark plasma sintering (SPS) device under argon protective gas at a temperature of 1650-1850°C for 2 hours to obtain a molten material, and then the molten material is cooled and solidified at a cooling rate of 80±5°C / min to obtain a ceramic solidified body;
[0043] 3) Crystallization heat treatment: The obtained ceramic solid body is crystallized and annealed in a muffle furnace at a temperature of 1250-1400°C for 6 hours to adjust the microstructure and eliminate stress, and is cooled to room temperature at a cooling rate of 30±5°C / min to obtain a nickel ferrite-based eutectic ceramic inert anode material.
[0044] After testing, the density of the material made in this embodiment is: 99.8%; the conductivity is 25S / cm; the mechanical properties are: bending strength 89MPa; thermal shock resistance: 1st residual strength ratio 102%; high temperature corrosion resistance: 15 microns.
[0045] Embodiment 2:
[0046] This embodiment is different from Embodiment 1 in that the raw materials used are 80 wt% NiFe2O4-based spinel powder, 20 wt% nickle-green stone powder, glycerol (accounting for 1 wt% of the total mass of NiFe2O4-based spinel powder and nickle-green stone powder) and water (5 times the total mass of NiFe2O4-based spinel powder and nickle-green stone powder).
[0047] After testing, the density of the material made in this embodiment is: 99.3%; the conductivity is 23S / cm; the mechanical properties are: bending strength 91MPa; thermal shock resistance: 1st residual strength ratio 98%; high temperature corrosion resistance: 17 microns.
[0048] Embodiment 3:
[0049] This embodiment is different from Embodiment 1 in that the raw materials used are 90wt% NiFe2O4-based spinel powder, 10wt% nickel oxide, propylene glycol (accounting for 4wt% of the total mass of NiFe2O4-based spinel powder and nickel green stone powder) and water (3 times the total mass of NiFe2O4-based spinel powder and nickel green stone powder).
[0050] After testing, the density of the material made in this embodiment is: 99.5%; the conductivity is 28S / cm; the mechanical properties are: bending strength 107MPa; thermal shock resistance: 1st residual strength ratio 117%; high temperature corrosion resistance: 5 microns.
[0051] The molten material obtained in the above embodiment can also be cast in an anode mold and then cooled under the same conditions, and the properties of the obtained material will not change.
Claims
1. A method for preparing a nickel ferrite-based eutectic ceramic inert anode material, Characterized in that the method include: Step 1, preparing a pre-sintered body: The mixed powder of NiFe2O4-based spinel powder and nickel green stone powder is mixed with a binder and granulated into 10-30 mesh granules; the granules are then pressed under a pressure of 100-200 MPa to obtain a green body; and the green body is pre-sintered for 2-5 hours at 1100-1300° C. in an inert gas atmosphere to obtain a pre-sintered body; Calculated as 100% by mass, the mass percentage of the NiFe2O4-based spinel is 80wt% to 90wt%, and the mass percentage of the nickel green stone is 10wt% to 20wt%; the binder is selected from one or a mixture of two or more of polyvinyl alcohol and polyethylene glycol, and the mass of the binder accounts for 0.5wt% to 2wt% of the mass of the mixed powder; The nickel green stone composition is: NiO accounts for 20wt% to 80wt%; CaO accounts for 0wt% to 20wt%; CeO2 accounts for 0wt% to 20wt%; ZrO2 accounts for 0wt% to 20wt%; Al2O3 accounts for 0wt% to 20wt%; V2O5 accounts for 0wt% to 20wt%; does not include the endpoint value 0; Step 2: Pre-sintered body melting and cooling solidification: The pre-sintered body is heated and melted in an inert gas atmosphere to make the pre-sintered body molten; then the molten material is cooled and solidified at a cooling rate of 1-100°C / min, or the molten material is cast and then cooled and solidified at a cooling rate of 1-100°C / min to obtain a ceramic solidified body; Step 3, heat treatment: The ceramic solid body obtained in step 2 is treated at a temperature of 1250-1400° C. for 2-6 hours, and then cooled to room temperature at a cooling rate of 1-50° C. / min to obtain a nickel ferrite-based eutectic ceramic inert anode material.
2. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that The NiFe2O4-based spinel composition is: NiFe2O4 accounts for 20wt% to 80wt%; ZnFe2O4 accounts for 0wt% to 20wt%; CuFe2O4 accounts for 0wt% to 20wt%; CoFe2O4 accounts for 0wt% to 20wt%; MnFe2O4 accounts for 0wt% to 20wt%; and does not include the endpoint value 0.
3. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that The particle size of the mixed powder is less than 100 meshes.
4. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that The method for preparing the mixed powder of NiFe2O4-based spinel powder and nickel green stone powder in step 1 is as follows: Ball milling a mixture of NiFe2O4-based spinel powder, nickel green stone powder, dispersant and water for 12-24 hours to obtain a ceramic slurry; then drying and grinding the ceramic slurry to obtain a mixed powder; The dispersant is selected from one or a mixture of two or more of ethanol, ethylene glycol and glycerol, and the mass of the dispersant accounts for 1wt%-5wt% of the total mass of the NiFe2O4-based spinel powder and the nickel green stone powder; The mass of the water is 3-5 times the total mass of the NiFe2O4-based spinel powder and the nickel green stone powder.
5. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that In step 2, the pre-sintered body is melted in an inert gas atmosphere at a temperature of 1650-1850° C. for 1-2 hours to make the pre-sintered body into a molten state.
6. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that The melting in step 2 is carried out by any one or a combination of arc melting, discharge plasma melting, laser suspension zone melting, optical floating zone melting, electron beam zone melting, high-frequency electromagnetic induction zone melting and energized Joule heat melting.
7. The method for preparing the nickel ferrite-based eutectic ceramic inert anode material according to claim 1, It is characterized in that The nickel ferrite-based eutectic ceramic inert anode material has a density of 99%-100%, a thermal shock resistance of 95%-120%, a mechanical property of 70-110 MPa, a high-temperature corrosion resistance of 5-50 microns, and a conductivity of 8-30 S / cm.
8. A method for preparing a nickel ferrite-based eutectic ceramic inert anode material, Characterized in that the method include: Step 1, preparing a pre-sintered body: The mixed powder of NiFe2O4-based spinel powder and NiO powder is mixed with a binder and granulated to form 10-30 mesh granules; the granules are then pressed under a pressure of 100-200 MPa to obtain a green body; and the green body is pre-sintered for 2-5 hours at 1100-1300° C. in an inert gas atmosphere to obtain a pre-sintered body; Calculated as 100% by mass, the mass percentage of the NiFe2O4-based spinel is 80wt% to 90wt%, and the mass percentage of NiO is 10wt% to 20wt%; the binder is selected from one or a mixture of two or more of polyvinyl alcohol and polyethylene glycol, and the mass of the binder accounts for 0.5wt% to 2wt% of the mass of the mixed powder; Step 2: Pre-sintered body melting and cooling solidification: The pre-sintered body is heated and melted in an inert gas atmosphere to make the pre-sintered body molten; then the molten material is cooled and solidified at a cooling rate of 1-100°C / min, or the molten material is cast and then cooled and solidified at a cooling rate of 1-100°C / min to obtain a ceramic solidified body; Step 3, heat treatment: The ceramic solid body obtained in step 2 is treated at a temperature of 1250-1400° C. for 2-6 hours, and then cooled to room temperature at a cooling rate of 1-50° C. / min to obtain a nickel ferrite-based eutectic ceramic inert anode material.