A lightweight fireproof exterior wall insulation decorative integrated board

By using phenolic resin, organic flame-retardant modified expanded graphite, modified rock wool, vitrified microbeads and other materials to make a fireproof insulation layer, and spraying real stone paint to form a decorative layer, the fireproof problem of the existing exterior wall insulation decorative integrated board has been solved. The problem of poor performance and average mechanical properties is achieved by achieving the effects of light weight, high strength and excellent fire resistance, and simplifying the installation process.

CN118307839BActive Publication Date: 2024-10-29HUNAN KERUI INTELLIGENT CONTROL AUTOMATION EQUIP CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410414216.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-29
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

Existing exterior wall insulation and decorative integrated panels have poor fire protection performance, average mechanical properties, and complex installation, which cannot meet the building's energy-saving needs.

Method used

The fireproof insulation layer is made of phenolic resin, organic flame-retardant modified expanded graphite, modified rock wool, vitrified microspheres and foaming agents, and is sprayed with real stone paint on its surface to form a decorative layer. The material is improved through modification treatment. compatibility and mechanical properties.

Benefits of technology

A lightweight, high-strength, and fire-proof integrated exterior wall insulation decorative panel has been realized, which has good insulation and fire-proof effects, simplifies the installation process, and reduces weight and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307839B_ABST
    Figure CN118307839B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of thermal insulation decorative panels, and specifically discloses a lightweight fireproof exterior wall thermal insulation decorative integrated panel, comprising a fireproof thermal insulation layer and a decorative layer, wherein the fireproof thermal insulation layer comprises phenolic resin, organic flame retardant modified expanded graphite, modified rock wool, vitrified microspheres, a foaming agent, a curing agent, and a dispersant, and the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, with vitrified microspheres and rock wool as skeleton supports, overlapping each other to form a three-dimensional staggered support network, and generating a cross-linked network structure between the organic flame retardant modified expanded graphite and the phenolic resin, thereby effectively improving the mechanical properties of the matrix, and the organic flame retardant and the expanded graphite act synergistically to have excellent fireproof performance, and the use of rock wool further ensures the thermal insulation performance of the integrated panel, and the real stone paint is used as the decorative layer, the integrated panel has the characteristics of lightness and fireproofing, the use process is simple, the cumbersome process is reduced, the practicability is strong, and the panel has broad application prospects and market potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal insulation decorative panels, in particular to a lightweight fireproof exterior wall thermal insulation decorative integrated panel. Background Art

[0002] Energy conservation and low carbon have been well controlled in industry and transportation, and the real estate sector is also being gradually planned. Building energy-saving materials are being vigorously promoted. Among them, the exterior wall insulation system is a key system in the field of building energy conservation, which has received more and more attention. It is required to install an insulation layer on the exterior wall to keep the indoor temperature at a higher temperature and reduce the waste of electricity and coal. Common exterior wall insulation decoration integrated panels usually include a two-layer structure of decorative panels and insulation panels. The insulation material is bonded to the decorative substrate with an organic adhesive. After the surface is sprayed with a decorative layer of paint, it is directly mounted on the wall. It has the advantages of environmental protection, energy saving, simple installation, time saving, rich decorative effects, and good pollution resistance. With the continuous improvement of the level of building energy conservation, the requirements for exterior wall insulation decoration integrated panels are also getting higher and higher. The performance of durability, beauty, light weight, high strength and fire resistance is also favored by more and more customers.

[0003] At present, the insulation layer of the thermal insulation decorative integrated panels on the market mostly uses materials such as rock wool, extruded board and polystyrene board. Rock wool has good fireproof performance, but high water absorption rate. The thermal insulation performance is greatly reduced after absorbing water. Materials such as extruded board and polystyrene board are flammable, have poor fireproof effect, and are easy to fall off, posing a great safety hazard. The calcium silicate board used in the decorative layer is prone to damage and cracking during the construction process, resulting in quality problems. The Chinese patent with application number CN201410156688.2 discloses a thermal insulation fireproof decorative panel, which includes a plywood layer, an insulation layer, a filler layer and a fixed layer. However, the wall with multiple panels installed occupies a large space, and the installation and operation are complicated, which cannot meet people's actual decoration operation needs. Application No. CN201610506291.0 discloses a modified phenolic resin composite thermal insulation material and a preparation method thereof. The material is composed of the following raw materials, calculated by weight: 30-70 parts of epoxy modified phenolic resin, 30-50 parts of coated expanded perlite, 10-20 parts of straw, 2-5 parts of adhesive, 1-3 parts of hydrophobic agent, 0.1-1 parts of curing agent, 0.1-1 parts of lubricant and 0.1-1 parts of toughening agent. The phenolic resin in the thermal insulation material has certain flame retardant properties. By adding a variety of inorganic materials, the material has the advantages of low thermal conductivity of organic thermal insulation materials and high strength and difficulty in burning of inorganic thermal insulation materials, and is light in weight. However, the combustion performance of the composite thermal insulation material can only reach B1 level, and the compatibility between the components is poor, and the mechanical properties are affected.

[0004] Therefore, there is an urgent need in the art to develop a thermal insulation decorative integrated panel material with simple structure, light weight, excellent mechanical properties and good fire resistance. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a lightweight fireproof exterior wall thermal insulation decorative integrated panel, which solves the problems of poor fireproof performance and general mechanical properties of the exterior wall thermal insulation decorative integrated panel.

[0007] (II) Technical solution

[0008] In order to achieve the above-mentioned purpose, the present invention discloses a lightweight fireproof exterior wall thermal insulation decorative integrated panel, comprising a fireproof thermal insulation layer and a decorative layer, wherein the fireproof thermal insulation layer comprises, by weight, 60-75 parts of phenolic resin, 5-9 parts of organic flame retardant modified expanded graphite, 2-4 parts of modified rock wool, 3-6 parts of glass microspheres, 1.5-2 parts of foaming agent, 8-15 parts of curing agent, and 0.1-0.3 parts of dispersant.

[0009] Preferably, the decorative layer is obtained by spraying real stone paint on the fireproof and heat-insulating layer.

[0010] Preferably, the spraying thickness of the decorative layer is 4-6 mm.

[0011] Preferably, the lightweight fireproof exterior wall insulation decorative integrated panel is prepared by the following steps:

[0012] Step 1, weighing phenolic resin, foaming agent, glass microspheres and dispersant according to the above mass parts, placing them in a mixer and stirring and mixing them evenly to obtain component A;

[0013] Step 2: weigh the organic flame retardant modified expanded graphite and modified rock wool according to the above mass parts, place them in a mixer, stir and mix them evenly, to obtain component B;

[0014] Step 3: After fully mixing component A and component B, add curing agent according to the above mass parts, stir for 60 minutes at a stirring rate of 400 r / min, perform compression molding, cool and shape, and obtain a fireproof and thermal insulation layer;

[0015] Step 4: Spray the real stone paint onto the fireproof insulation layer, dry it naturally for 48 hours, form a decorative layer on the surface of the fireproof insulation layer, and obtain a lightweight fireproof exterior wall insulation decorative integrated board.

[0016] Preferably, the blowing agent is n-pentane.

[0017] Preferably, the curing agent is hexamethyltetramine.

[0018] Preferably, the dispersant is polyethylene wax.

[0019] Preferably, the organic flame retardant modified expanded graphite is prepared by the following steps:

[0020] S1. Prepare 90% ethanol aqueous solution, add expanded graphite (EG) and γ-aminopropyltriethoxysilane, stir for 2-3 hours, add 4-carboxyphenylboric acid, dicyclohexylcarbodiimide (DCC) and 4-dimethylaminopyridine (DMAP), react at 20-35° C. for 3-6 hours, and after the reaction is completed, wash with anhydrous ethanol and dry to obtain phenylboric acid modified expanded graphite;

[0021] S2. 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is modified with methacryloxypropyltrimethoxysilane to obtain silylated phosphaphenanthrene. In a nitrogen atmosphere, diethylene glycol dimethyl ether, silylated phosphaphenanthrene, phenylboric acid modified expanded graphite and aqueous hydrochloric acid solution are mixed evenly, heated, and reacted at 120-140°C for 3-5h. After the reaction is completed, the mixture is washed with acetone and dried to obtain organic flame retardant modified expanded graphite.

[0022] Preferably, the mass ratio of expanded graphite, γ-aminopropyltriethoxysilane, 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine in S1 is 100:35-42:138-165:35-55:18-25.

[0023] Preferably, the hydrochloric acid aqueous solution in S2 is a hydrochloric acid aqueous solution with a mass concentration of 3%.

[0024] Preferably, the specific synthesis steps of the silanized phosphophenanthrene derivative in S2 are as follows: diethylene glycol dimethyl ether and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide are stirred and mixed, the temperature is raised to 80°C, and after mixing evenly, methacryloxypropyltrimethoxysilane and azobisisobutyronitrile are added, and stirred and mixed, wherein the mass ratio of the added diethylene glycol dimethyl ether, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, methacryloxypropyltrimethoxysilane and azobisisobutyronitrile is 1200:100:98:0.8, the temperature is raised, and the reaction is carried out at 80°C for 24 hours. After the reaction is completed, the silanized phosphophenanthrene is washed with cyclohexane and dried to obtain the silylated phosphophenanthrene.

[0025] Preferably, the mass ratio of diethylene glycol dimethyl ether, silylated phosphine phenanthrene, phenylboronic acid modified expanded graphite and hydrochloric acid aqueous solution in S2 is 1500-1800:24-32:100:40-50.

[0026] Preferably, the modified rock wool is prepared by the following steps:

[0027] The rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane were stirred and mixed evenly, and then ultrasonically dispersed at a frequency of 1200-1400 Hz for 30 minutes, heated, soaked at 130-140° C. for 2-3 hours, cooled, filtered, washed with deionized water, and dried to obtain modified rock wool.

[0028] Preferably, in the preparation process of the modified rock wool, the mass ratio of the rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane is 100:800-1000:20-50:15-60.

[0029] (III) Beneficial technical effects

[0030] (1) In the present invention, γ-aminopropyl triethoxysilane is used to modify expanded graphite, amino groups and silanes are introduced on the surface of expanded graphite, and amidation reaction occurs between the amino groups introduced on the surface of expanded graphite and the carboxyl groups on 4-carboxyl phenylboronic acid to obtain phenylboronic acid modified expanded graphite, and addition reaction occurs between the PH bond on 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and the carbon-carbon double bond on methacryloxypropyl trimethoxysilane to obtain silylated phosphophophanate, and Si-OCH3 on silylated phosphophanate is hydrolyzed into Si-OH, and dehydrated and condensed with B-OH on phenylboronic acid modified expanded graphite to obtain organic flame retardant modified expanded graphite. Sodium methyl silicate and dodecyl trimethoxysilane are used to modify rock wool, and a large amount of silanes are introduced. The two act synergistically to reduce the adhesion to water, and the alkyl hydrophobic long chain has an excellent hydrophobic effect, which can form a hydrophobic layer on the surface of rock wool, and the obtained modified rock wool has a good waterproof effect.

[0031] (2) In the present invention, expanded graphite has the advantages of light weight, thin layer, easy processing, etc., and expanded graphite has excellent thermal insulation performance, which is mainly due to its good thermal resistance and low thermal conductivity, so that the speed of heat propagation in the matrix is ​​slow, thereby effectively blocking the transfer of heat. In addition, the high porosity of expanded graphite also contributes to its thermal insulation performance. The air in the pores also has thermal resistance, which can further prevent the transfer of heat. It can be used as a thermal insulation material for the exterior wall of a building. At the same time, expanded graphite can expand rapidly during the combustion process of the matrix, effectively isolate heat and oxygen, and prevent the escape of flammable volatile substances, and has excellent fireproof and heat-insulating effects. Vitrified microspheres are an inorganic lightweight thermal insulation material, and their particles are irregularly spherical, and their interior is a porous cavity structure, while the outer surface is closed and smooth, and has excellent properties such as light weight, thermal insulation, fire resistance, high temperature resistance, aging resistance, and low water absorption. It can prevent the decorative layer from cracking, play the role of coarse aggregate, and reduce the weight of the integrated board. The phosphorus-containing flame retardant introduced on the expanded graphite can produce a large amount of acidic substances during the combustion process, and synergize with a large amount of silicon elements and expanded graphite to form a denser carbon layer on the surface of the matrix to prevent the combustion reaction. The large amount of amino groups introduced during the reaction can produce non-flammable nitrogen-containing gas during the combustion process, which effectively dilutes the concentration of oxygen in the combustion system, slows down the combustion reaction, and further achieves the purpose of fire prevention. The modification of expanded graphite effectively avoids agglomeration and can be better dispersed in the matrix. As a highly efficient thermal insulation material, rock wool has slender fibers and is a non-combustible and fire-resistant thermal insulation material. After being modified by silane, it has excellent hydrophobic properties and greatly improves its dispersibility. The imino group in the organic flame retardant modified expanded graphite can generate hydrogen bonds with the phenolic resin matrix, and with the glass microspheres and rock wool as the skeleton, it plays a good supporting role in the integrated board, overlaps with the organic flame retardant modified expanded graphite and phenolic resin to form a three-dimensional staggered support network, and produces a cross-linked network structure, which effectively improves the mechanical properties of the matrix. The excellent compatibility reduces the pores between the raw materials, avoids self-accumulation, reduces heat transfer, and further improves the thermal insulation performance of the integrated board. Furthermore, the use of real stone paint as a decorative layer has the characteristics of light weight and fire resistance, simple use process, reduces cumbersome processes, strong practicality, and has broad application prospects and market potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 Flow chart for preparing lightweight fireproof exterior wall insulation decorative integrated panels;

[0034] Figure 2 Schematic diagram of the structure of synthesized phenylboric acid modified expanded graphite. DETAILED DESCRIPTION

[0035] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0036] Example 1

[0037] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 1.5 mm, wherein the fireproof thermal insulation layer comprises, by weight, 60 parts of phenolic resin, 5 parts of organic flame retardant modified expanded graphite, 2 parts of modified rock wool, 3 parts of glass microspheres, 1.5 parts of foaming agent n-pentane, 8 parts of curing agent hexamethyltetramine, and 0.1 part of dispersant polyethylene wax.

[0038] The organic flame retardant modified expanded graphite is prepared by the following steps:

[0039] S1, prepare 90% ethanol aqueous solution, add expanded graphite and γ-aminopropyltriethoxysilane, stir for 2h, add 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, wherein the mass ratio of expanded graphite, γ-aminopropyltriethoxysilane, 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 100:35:138:35:18, react at 20°C for 6h, after the reaction is completed, wash with anhydrous ethanol, dry, and obtain phenylboric acid modified expanded graphite;

[0040] S2. In a nitrogen atmosphere, diethylene glycol dimethyl ether, silylated phosphine phenanthrene, phenylboric acid modified expanded graphite and hydrochloric acid aqueous solution in a mass ratio of 1500:24:100:40 are mixed evenly, heated, and reacted at 120°C for 5 hours. After the reaction is completed, the mixture is washed with acetone and dried to obtain organic flame retardant modified expanded graphite.

[0041] The modified rock wool is prepared by the following steps:

[0042] Rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane in a mass ratio of 100:800:20:15 were stirred and mixed evenly, and then ultrasonically dispersed at a frequency of 1200 Hz for 30 minutes, heated, immersed at 130° C. for 3 hours, cooled, filtered, washed with deionized water, and dried to obtain modified rock wool.

[0043] Example 2

[0044] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 5 mm, wherein the fireproof thermal insulation layer comprises, by weight, 65 parts of phenolic resin, 6 parts of organic flame retardant modified expanded graphite, 2.5 parts of modified rock wool, 4 parts of glass microspheres, 1.6 parts of foaming agent n-pentane, 10 parts of curing agent hexamethyltetramine, and 0.2 parts of dispersant polyethylene wax.

[0045] The organic flame retardant modified expanded graphite is prepared by the following steps:

[0046] S1, prepare 90% ethanol aqueous solution, add expanded graphite and γ-aminopropyltriethoxysilane, stir for 2.5h, add 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, wherein the mass ratio of expanded graphite, γ-aminopropyltriethoxysilane, 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 100:40:150:45:21, react at 30°C for 4h, after the reaction is completed, wash with anhydrous ethanol, dry, and obtain phenylboric acid modified expanded graphite;

[0047] S2. In a nitrogen atmosphere, diethylene glycol dimethyl ether, silylated phosphine phenanthrene, phenylboronic acid modified expanded graphite and hydrochloric acid aqueous solution in a mass ratio of 1600:30:100:45 are mixed evenly, heated, and reacted at 130° C. for 4 hours. After the reaction is completed, the mixture is washed with acetone and dried to obtain an organic flame retardant modified expanded graphite.

[0048] The modified rock wool is prepared by the following steps:

[0049] Rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane in a mass ratio of 100:900:40:45 were stirred and mixed evenly, and then ultrasonically dispersed at a frequency of 1300 Hz for 30 minutes, heated, immersed at 135° C. for 2.5 hours, cooled, filtered, washed with deionized water, and dried to obtain modified rock wool.

[0050] Example 3

[0051] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 5 mm, wherein the fireproof thermal insulation layer comprises, by weight, 70 parts of phenolic resin, 8 parts of organic flame retardant modified expanded graphite, 3.5 parts of modified rock wool, 5 parts of glass microspheres, 1.8 parts of foaming agent n-pentane, 12 parts of curing agent hexamethyltetramine, and 0.2 parts of dispersant polyethylene wax.

[0052] The preparation method of the organic flame retardant modified expanded graphite and modified rock wool is the same as the preparation method of Example 2.

[0053] Example 4

[0054] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 6 mm, wherein the fireproof thermal insulation layer comprises, by mass, 75 parts of phenolic resin, 9 parts of organic flame retardant modified expanded graphite, 4 parts of modified rock wool, 6 parts of glass microspheres, 2 parts of foaming agent n-pentane, 15 parts of curing agent hexamethyltetramine, and 0.3 parts of dispersant polyethylene wax.

[0055] The organic flame retardant modified expanded graphite is prepared by the following steps:

[0056] S1, prepare 90% ethanol aqueous solution, add expanded graphite and γ-aminopropyltriethoxysilane, stir for 3h, add 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, wherein the mass ratio of expanded graphite, γ-aminopropyltriethoxysilane, 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine is 100:42:165:55:25, react at 35°C for 3h, after the reaction is completed, wash with anhydrous ethanol, dry, and obtain phenylboric acid modified expanded graphite;

[0057] S2. In a nitrogen atmosphere, diethylene glycol dimethyl ether, silylated phosphine phenanthrene, phenylboric acid modified expanded graphite and hydrochloric acid aqueous solution in a mass ratio of 1800:32:100:50 are mixed evenly, heated, and reacted at 140°C for 3h. After the reaction is completed, the mixture is washed with acetone and dried to obtain organic flame retardant modified expanded graphite.

[0058] The modified rock wool is prepared by the following steps:

[0059] Rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane in a mass ratio of 100:1000:50:60 were stirred and mixed evenly, and then ultrasonically dispersed at a frequency of 1400 Hz for 30 minutes, heated, immersed at 140°C for 2 hours, cooled, filtered, washed with deionized water, and dried to obtain modified rock wool.

[0060] Comparative Example 1

[0061] A lightweight fireproof exterior wall insulation decorative integrated panel comprises a fireproof insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof insulation layer, and the spraying thickness is 5 mm, wherein the fireproof insulation layer comprises, by weight, 70 parts of phenolic resin, 8 parts of expanded graphite, 3.5 parts of modified rock wool, 5 parts of glass microspheres, 1.8 parts of foaming agent n-pentane, 12 parts of curing agent hexamethyltetramine, and 0.2 parts of dispersant polyethylene wax.

[0062] The preparation method of the modified rock wool is the same as that of Example 2.

[0063] Comparative Example 2

[0064] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 5 mm, wherein the fireproof thermal insulation layer comprises, by weight, 70 parts of phenolic resin, 8 parts of organic flame retardant modified expanded graphite, 3.5 parts of rock wool, 5 parts of glass microspheres, 1.8 parts of foaming agent n-pentane, 12 parts of curing agent hexamethyltetramine, and 0.2 parts of dispersant polyethylene wax.

[0065] The preparation method of the organic flame retardant modified expanded graphite is the same as that of Example 2.

[0066] Comparative Example 3

[0067] A lightweight fireproof exterior wall thermal insulation decorative integrated panel comprises a fireproof thermal insulation layer and a decorative layer, wherein the decorative layer is obtained by spraying real stone paint on the fireproof thermal insulation layer, and the spraying thickness is 5 mm, wherein the fireproof thermal insulation layer comprises, by weight, 70 parts of phenolic resin, 8 parts of expanded graphite, 3.5 parts of rock wool, 5 parts of vitrified microspheres, 1.8 parts of foaming agent n-pentane, 12 parts of curing agent hexamethyltetramine, and 0.2 parts of dispersant polyethylene wax.

[0068] The expanded graphite used in the embodiments and comparative examples of the present invention was purchased from Qingdao Graphite Co., Ltd., wherein the expansion rate of the expanded graphite is 200 mL / g and the particle size is 50 mesh; the vitrified microspheres were purchased from Beijing Juneng Xingye Technology Development Co., Ltd., which are expanded vitrified microspheres; the rock wool was purchased from Rockaway Fireproof Insulation Materials Guangzhou Co., Ltd., and the acidity coefficient was 1.70; the phenolic resin was purchased from Hangmo New Materials Group Co., Ltd., which is a brown-red liquid with a viscosity (25°C) of 1500-3000 mPa·s, a solid content of 70-85%, and free phenol <5%; the real stone paint was from Baorunda New Materials Co., Ltd.

[0069] The lightweight fireproof exterior wall insulation decorative integrated panels prepared in Examples 1-4 and Comparative Examples 1-3 were used as samples for performance tests, and the relevant tests are as follows:

[0070] (1) Fire performance test: Test the samples in accordance with the national standard GB 8624-2012 “Classification of Combustion Performance of Building Materials and Products” and record the combustion performance level;

[0071] (2) Thermal insulation performance test: Test the samples according to the national standard GB / T 10294-2008 "Determination of steady-state thermal resistance and related properties of thermal insulation materials - guarded hot plate method" and record the thermal conductivity;

[0072] (3) Mechanical properties test: The test was carried out with reference to the national standard GB / T 25975-2018 "Rock wool products for external thermal insulation of building exterior walls". The tensile strength and compressive strength were tested on the LDW-5000 electronic universal testing machine. The test results are shown in Table 1:

[0073] Table 1

[0074]

[0075] According to the test results in Table 1, Examples 1-4 have excellent fireproof and heat preservation properties and excellent mechanical properties. The combustion performance level of the samples corresponding to Examples 1-4 can reach A1, and the thermal conductivity of the sample corresponding to Example 4 can be as low as 0.026 W·m -1 ·K -1 , the compression strength can reach 3.01MPa, and the tensile strength corresponding to Example 3 can reach 3.04MPa. In Comparative Example 1, the expanded graphite was not modified, no phosphorus-containing flame retardant was introduced, and the dispersion performance was poor, the compatibility between the phenolic resin and other raw materials was greatly reduced, and the comprehensive performance was reduced; in Comparative Example 2, the rock wool was not modified, the dispersion was also reduced, and the thermal conductivity was greatly affected, which was 0.068W·m -1 ·K -1 In Comparative Example 3, neither the expanded graphite nor the rock wool was modified, and the comprehensive performance was greatly reduced, and the fire resistance, thermal insulation and mechanical properties were poor.

[0076] Although the embodiments of the present invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that all equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A lightweight fireproof exterior wall insulation decorative integrated board, It is characterized in that It includes a fireproof and thermal insulation layer and a decorative layer, wherein the fireproof and thermal insulation layer includes, by weight, 60-75 parts of phenolic resin, 5-9 parts of organic flame retardant modified expanded graphite, 2-4 parts of modified rock wool, 3-6 parts of vitrified microspheres, 1.5-2 parts of foaming agent, 8-15 parts of curing agent, and 0.1-0.3 parts of dispersant; The decorative layer is obtained by spraying real stone paint on the fireproof and heat-insulating layer; The lightweight fireproof exterior wall thermal insulation decorative integrated board is prepared by the following steps: Step 1, weighing phenolic resin, foaming agent, glass beads and dispersant according to the above mass parts, placing them in a mixer and stirring and mixing them evenly to obtain component A; Step 2: weigh the organic flame retardant modified expanded graphite and modified rock wool according to the above mass parts, place them in a mixer, stir and mix them evenly, to obtain component B; Step 3: After component A and component B are fully mixed, a curing agent is added according to the above mass parts, and the mixture is stirred at a stirring rate of 400 r / min for 60 min, and compression molding is performed to cool and shape the mixture to obtain a fireproof and thermal insulation layer; Step 4: spray the real stone paint onto the fireproof and thermal insulation layer, dry it naturally for 48 hours, form a decorative layer on the surface of the fireproof and thermal insulation layer, and obtain a lightweight fireproof exterior wall thermal insulation decorative integrated board; The organic flame retardant modified expanded graphite is prepared by the following steps: S1. Prepare 90% ethanol aqueous solution, add expanded graphite and γ-aminopropyltriethoxysilane, stir for 2-3 hours, add 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine, react at 20-35° C. for 3-6 hours, and after the reaction is completed, wash with anhydrous ethanol and dry to obtain phenylboric acid modified expanded graphite; S2. Modify 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide with methacryloxypropyltrimethoxysilane to obtain silylated phosphaphenanthrene, and evenly mix diethylene glycol dimethyl ether, silylated phosphaphenanthrene, phenylboronic acid-modified expanded graphite and hydrochloric acid aqueous solution in a nitrogen atmosphere, raise the temperature, and react at 120-140° C. for 3-5 hours. After the reaction is completed, wash with acetone and dry to obtain organic flame-retardant modified expanded graphite; The modified rock wool is prepared by the following steps: The rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane were stirred and mixed evenly, and then ultrasonically dispersed at a frequency of 1200-1400 Hz for 30 minutes, heated, soaked at 130-140° C. for 2-3 hours, cooled, filtered, washed with deionized water, and dried to obtain modified rock wool.

2. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The mass ratio of expanded graphite, γ-aminopropyltriethoxysilane, 4-carboxyphenylboric acid, dicyclohexylcarbodiimide and 4-dimethylaminopyridine in S1 is 100:35-42:138-165:35-55:18-25.

3. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The specific synthesis steps of the alkenyl phosphinophenanthrene derivative in S2 are as follows: diethylene glycol dimethyl ether and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide are stirred and mixed, the temperature is raised to 80°C, and after mixing evenly, methacryloxypropyltrimethoxysilane and azobisisobutyronitrile are added, and stirred and mixed, wherein the mass ratio of the added diethylene glycol dimethyl ether, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, methacryloxypropyltrimethoxysilane and azobisisobutyronitrile is 1200:100:98:0.8, the temperature is raised, and the reaction is carried out at 80°C for 24 hours. After the reaction is completed, the silylated phosphinophenanthrene is washed with cyclohexane and dried to obtain the alkenyl phosphinophenanthrene.

4. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The mass ratio of diethylene glycol dimethyl ether, silylated phosphine phenanthrene, phenylboronic acid modified expanded graphite and hydrochloric acid aqueous solution in S2 is 1500-1800:24-32:100:40-50.

5. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The mass ratio of the rock wool, deionized water, sodium methyl silicate and dodecyltrimethoxysilane is 100:800-1000:20-50:15-60.

6. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The spraying thickness of the decorative layer is 4-6 mm.

7. A lightweight fireproof exterior wall insulation decorative integrated board according to claim 1, It is characterized in that The foaming agent is n-pentane, the curing agent is hexamethyltetramine, and the dispersant is polyethylene wax.

Citation Information

Patent Citations

  • Heat preservation type fireproof decorative plate

    CN103899064A

  • Modified phenolic resin composite thermal insulation material and preparation method thereof

    CN106046671A

  • Fire prevention, thermal insulation and decoration integrated board

    CN102011470A

  • Heat insulation fireproof wallboard

    CN106013594A

  • Method for preparing modified expandable graphite / polypropylene flame-retardant material

    CN106397984A