A nickel-iron-cobalt trimetallic nanoarray electrocatalyst, method and application thereof in electrocatalytic oxidation of 5-hydroxymethylfurfural

The hydrothermal pretreatment and calcination activation of nickel-iron-cobalt trimetal nanoarray electrocatalysts are formed, which solves the problem of insufficient electronic structure regulation of nickel-based catalysts and achieves efficient and stable HMF oxidation to FDCA significantly improves conversion and yield.

CN118385603BActive Publication Date: 2024-11-08AGRO ENVIRONMENTAL PROTECTION INST OF MIN OF AGRI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410804248.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-11-08
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

The existing technology lacks the internal mechanism of the regulation of electronic structure of nickel-based catalysts. The absorption and binding of OH plays a key role in HMF oxidation, but the lack of exploration of the absorption mechanism, active sites and absorption groups in the molecule, limiting HMF Convert to FDCA efficiency.

Method used

Using nickel-iron-cobalt trimetal nanoarray electrocatalyst, the foam nickel foam is pretreated and calcined and activated by hydrothermal method to form a layered nanosheet structure, increasing the surface area and active site exposure of the catalyst, improving electron transfer efficiency, and Catalytic oxidation of 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid under electrochemical conditions.

Benefits of technology

Achieve rapid selective oxidation of HMF under mild conditions, obtaining lower starting potential and high current density, the catalyst has excellent stability and high conversion rate, and the FDCA yield and Faraday efficiency are significantly improved, which is far superior to traditional LDHs and nickel. base catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118385603B_ABST
    Figure CN118385603B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electrochemical catalytic oxidation materials, discloses a nickel-iron-cobalt trimetallic nanoarray electrocatalyst, method and application of electrocatalytic oxidation of 5-hydroxymethylfurfural, including the following steps: pretreatment of nickel foam; ultrasonically mixing soluble nickel salt, soluble iron salt and soluble cobalt salt into ultrapure water, adding urea and NH4F ultrasonically mixed uniformly, and obtaining a mixed solution; vertically placing the pretreated pure nickel foam into an autoclave, adding a combined solution, placing in an oven for sealing reaction, and after the reactor is cooled, successively using ethanol and ultrapure water to clean the nickel foam, obtaining a layered nanosheet array precursor; placing in a muffle furnace for calcination activation, and obtaining an electrocatalyst after the reaction chamber is cooled. The electrocatalyst of the present invention can complete the rapid selective oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid under mild conditions, and obtain a lower starting potential and a higher current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical catalytic oxidation materials, and in particular to a nickel-iron-cobalt trimetallic nanoarray electrocatalyst, a method and an application thereof in the electrocatalytic oxidation of 5-hydroxymethylfurfural. Background Art

[0002] The increasing depletion of fossil fuel reserves and the increasing environmental awareness have triggered the pursuit of renewable resources. Biomass is the most abundant renewable resource on earth and is an ideal candidate for the production of value-added chemicals and sustainable energy. 5-Hydroxymethylfurfural (HMF) is an important biomass-based platform chemical used to synthesize compounds with high added value. 2,5-Furandicarboxylic acid (FDCA), an oxidation product of HMF, has a wide range of applications and huge market demand because it can be used as a monomer for bio-based polymers to replace the petroleum derivative terephthalic acid (TPA). Traditionally, FDCA can be obtained from HMF conversion by thermal catalysis, biocatalysis, etc., but the former has high reaction requirements (high temperature and pressure) and the latter requires a long fermentation period. With its low energy consumption and relatively mild operating conditions, the electrocatalytic oxidation of HMF to FDCA has become a more promising method to deal with this transformation in recent years.

[0003] Developing ideal electrocatalysts is a key step to promote efficient HMF conversion. In general, noble metals have severely limited their commercial application due to the high cost of raw materials. An increasing number of transition metal catalysts, including oxides, hydroxides, nitrides, phosphides, and sulfides of transition metals (Ni, Fe, and Co), have been shown to have higher electrocatalytic activity than rare noble metal catalysts. The nanosheet structure of transition metal layered double hydroxides (LDHs) has a large specific surface area and high exposure of activation sites, which can provide more charge transfer channels for electrolysis reactions. Among them, nickel-based catalysts are considered to be one of the most promising non-noble metal catalysts for HMFOR. According to recent studies, the electronic structure in LDHs can be regulated by introducing transition metals (Co, Fe, and Mn) into Ni-based oxides or (oxy)hydroxides to generate trimetallic composites. This significantly improves the electrocatalytic ability for HMF oxidation. However, there is a lack of in-depth research on the intrinsic mechanism of regulating the electronic structure of Ni-based catalysts. In addition, OH - The absorption and binding of play a key role in activating CH / OH nodes or forming high-value activation phases and are the key factors affecting HMFOR, but the lack of exploration of the absorption mechanism, active sites, and absorption groups in the molecule is still unclear. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a nickel-iron-cobalt trimetallic nanoarray electrocatalyst, a method and an application thereof in the electrocatalytic oxidation of 5-hydroxymethylfurfural.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A nickel-iron-cobalt trimetallic nanoarray electrocatalyst, the preparation method of which comprises the following steps:

[0007] (1) Pretreatment of nickel foam: The nickel foam is washed with HCl, ethanol and ultrapure water in sequence to remove oxides, oil stains and residual HCl to obtain pure nickel foam;

[0008] (2) ultrasonically mixing soluble nickel salt, soluble iron salt and soluble cobalt salt into ultrapure water, and then adding urea and NH4F and ultrasonically mixing them uniformly to obtain a mixed solution;

[0009] (3) vertically placing the pretreated pure nickel foam into a high-pressure reactor, adding the mixed solution prepared in step (2), and sealing the reaction in an oven. After the high-pressure reactor is cooled, the nickel foam is washed with ethanol and ultrapure water in turn to obtain a layered nanosheet array precursor;

[0010] (4) The precursor obtained in step (3) is placed in a muffle furnace for calcination and activation, and a nickel-iron-cobalt trimetallic nanoarray electrocatalyst is obtained after the reaction chamber is cooled.

[0011] Furthermore, the thickness of the nickel foam NF in step (1) is 1.5 mm, which is cut into a size of 1×2 cm (mass is 0.06 g), the concentration of HCl is 1 mol / L, the volume concentration of ethanol is 95%, and 5-10 mL of ultrapure water is added for every 0.06 g of nickel foam.

[0012] Furthermore, the soluble nickel salt in step (2) is at least one of nickel chloride hexahydrate, nickel sulfate hexahydrate, and nickel nitrate hexahydrate (Ni(NO3)2·6H2O), the soluble iron salt is at least one of ferric chloride hexahydrate, ferric sulfate nonahydrate, and ferric nitrate nonahydrate (Fe(NO3)3·9H2O), and the soluble cobalt salt is at least one or more of cobalt chloride hexahydrate, cobalt sulfate hexahydrate, and cobalt nitrate hexahydrate (Co(NO3)2·6H2O).

[0013] Furthermore, the molar ratio of the soluble nickel salt, the soluble iron salt and the soluble cobalt salt in step (2) is 3:1:2, the amount of water injected into each 0.6 mmol total amount of the soluble nickel salt, the soluble iron salt and the soluble cobalt salt is 10 mL, and the concentration of urea and NH4F is 1 mmol.

[0014] Furthermore, the hydrothermal pretreatment temperature of the high-pressure reactor in step (3) is 150° C., and the insulation time is 6 h.

[0015] Furthermore, the temperature of the calcination activation in step (4) is 300°C and the time is 2 h.

[0016] Application of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as described above in the electrocatalytic oxidation of 5-hydroxymethylfurfural.

[0017] Application of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as described above in the oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid.

[0018] The method for electrocatalytically oxidizing 5-hydroxymethylfurfural using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as described above comprises the following steps:

[0019] A three-electrode system is prepared using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as a working electrode, an Ag / AgCl electrode as a reference electrode, a graphite carbon rod as a counter electrode, and a KOH solution as an electrolyte; 5-hydroxymethylfurfural is dissolved in the electrolyte, and an external voltage is applied to the three-electrode system to perform an electrochemical catalytic oxidation reaction.

[0020] Furthermore, the KOH electrolyte concentration is 1 mol, and the 5-hydroxymethylfurfural concentration is 20 mM; the electrocatalytic oxidation reaction is carried out by a constant potential scanning method with an additional voltage of 1.0 V vs. RHE~1.8 V vs. RHE, the reaction time is 0.25 h~10 h, and the reaction temperature is 10°C~30°C.

[0021] The advantages and positive effects achieved by the present invention are:

[0022] 1. The present invention pre-treats nickel foam by hydrothermal method, grows nanosheets in situ, and activates them by calcination in the later stage to obtain nickel-iron-cobalt trimetallic nanoarray electrocatalyst, thereby enhancing catalytic performance. The catalyst of the present invention can complete the rapid selective oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid under mild conditions, and obtain a lower starting potential and a higher current density.

[0023] 2. The wrinkled nanosheet structure constructed by the present invention has excellent electrocatalytic performance. It can be seen from the results of the embodiment that 50~100 mA cm is achieved at a relatively low starting potential (1.26~1.43V vs. REH). -2 The prepared nickel-iron-cobalt trimetallic nanoarray electrocatalyst has excellent stability. In 5 consecutive cycles, the conversion rate of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid can reach 99.7~100%, the yield of 2,5-furandicarboxylic acid is 97.3~98.7%, and the Faraday efficiency is 96.8~98.5%, which is much better than most reported LDHs and nickel-based catalysts.

[0024] 3. The present invention shows through characterization that the doping of Fe and Co increases the electrochemically active surface area, accelerates the efficiency of electron transfer, and exposes more active sites. The present invention prepares a cost-effective ternary LDHs electrocatalyst with excellent electrocatalytic performance and stability, which promotes the development of green and environmentally friendly electrochemical methods for converting HMF to FDCA.

[0025] 4. The present invention pre-treats nickel foam by a hydrothermal method, grows a layered nanosheet structure in situ, increases the surface area of ​​the catalyst, and performs calcination activation in the later stage to increase the exposure of active sites. The present invention not only increases the active surface area of ​​the catalyst by in-situ growing a metal nanosheet structure on nickel foam, but also improves the electron transfer efficiency, has a low starting potential, and has high HMF conversion efficiency and FDCA yield. The tri-metal nanoarray catalyst of the present invention has excellent stability and durability, can be recycled, and has great economic and environmental value. The results of the embodiment show that the catalyst has excellent electrocatalytic performance: in a 1.0 M KOH solution, when the current density is 10 mA cm -2 The initial potential was only 1.26 V vs. RHE. After five consecutive cycles, the conversion of HMF was 99.7-100%, the yield of FDCA was 97.3-98.7%, and the Faradaic efficiency was 96.8-98.5%.

[0026] 5. The present invention successfully prepared a nickel-iron-cobalt trimetallic nanoarray electrocatalyst by hydrothermal pretreatment and post-pyrolysis carbonization. FDCA was prepared by electrochemical catalytic oxidation of HMF. The hydrothermal pretreatment was carried out at 150°C in a high-pressure reactor for 6 hours, followed by calcination at 300°C in a muffle furnace for 2 hours. In the three-electrode system, the nickel-iron-cobalt trimetallic nanoarray electrocatalyst was used as the working electrode, the Ag / AgCl electrode was used as the reference electrode, the graphite carbon rod was used as the counter electrode, and the 1M KOH solution was used as the electrolyte to prepare a three-electrode system in an H-type electrolytic cell; 5-hydroxymethylfurfural was dissolved in the electrolyte, and an external voltage was applied to the three-electrode system for electrochemical catalytic oxidation reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the SEM of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst in Example 1 of the present invention;

[0028] Figure 2 TEM spectrum of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst in Example 1 of the present invention;

[0029] Figure 3The nickel-iron-cobalt trimetallic nanoarray electrocatalyst in Example 1 of the present invention was subjected to a 1 M KOH solution containing or not containing 20 mM HMF at 50 mV s -1 LSV curve of rate scan;

[0030] Figure 4 It is a comparison chart of the conversion rate of HMF on the electrode, the yield of FDCA and the FE of FDCA in Example 1 and Comparative Examples 2-3 of the present invention at a voltage of 1.45 V vs. RHE;

[0031] Figure 5 This is a stability test diagram of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst in Example 1 of the present invention after 5 consecutive cycles of electrolysis;

[0032] Figure 6 The CV spectra of Comparative Examples 4 to 10 in the present invention were obtained under the conditions of a fixed HMF concentration of 20 mM and a changed KOH concentration;

[0033] Figure 7 The CV spectra of Comparative Examples 11 to 17 of the present invention were obtained under the conditions of a fixed 1 M KOH concentration and a changed HMF concentration;

[0034] Figure 8 HPLC spectra of different reaction times carried out under the conditions of fixed 1 M KOH concentration, 20 mM HMF concentration and 1.5 V vs. RHE voltage in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the embodiments. The following embodiments are descriptive rather than restrictive, and the protection scope of the present invention cannot be limited by the following embodiments.

[0036] The various experimental operations involved in the specific embodiments are all routine techniques in the art. For parts not specially annotated in this document, ordinary technicians in the art can implement them by referring to various commonly used reference books, scientific and technological literature or related instructions, manuals, etc. before the filing date of this invention.

[0037] The present invention cuts the nickel foam and then performs hydrothermal and calcination in sequence to obtain an in-situ grown nanosheet structure electrocatalyst. In the present invention, the in-situ grown substrate can be nickel foam, or can be a substrate such as copper foam, copper sheet, and carbon cloth. The present invention uses a porous material as a substrate to achieve electrocatalytic oxidation of HMF to prepare FDCA, save resources, save energy and protect the environment, and meet the requirements of sustainable development.

[0038] In the present invention, the target thickness of the nickel foam is preferably 0.5-2.5 mm, more preferably 1-1.5 mm; the target size is preferably (1-2)×(1-2) cm, more preferably 1×2 cm, and the crushing method is preferably cutting.

[0039] In the present invention, the temperature of the hydrothermal carbonization is preferably 120-180 r / min, more preferably 150 r / min, and the holding time is preferably 4-12 h, more preferably 6-8 h, and further preferably 6 h; the present invention has no special requirements for the hydrothermal equipment, and a high-pressure reactor familiar to those skilled in the art can be used. The amount of water added for the hydrothermal pretreatment is preferably 8-15 mL, more preferably 10 mL. The present invention in situ grows a layered wrinkled nanosheet structure on nickel foam through hydrothermal pretreatment, thereby increasing the specific surface area of ​​the electrocatalyst and the content of oxygen-containing functional groups, and obtaining more active sites.

[0040] In the present invention, the soluble metal salt preferably includes one or more of a soluble nickel salt, a soluble iron salt, and a soluble cobalt salt; the soluble nickel salt preferably includes one or both of nickel nitrate and nickel chloride; the soluble iron salt preferably includes one or both of ferric nitrate and ferric chloride; the soluble cobalt salt preferably includes one or both of cobalt nitrate and cobalt chloride.

[0041] In the present invention, after the hydrothermal treatment, the obtained carbonized product is preferably subjected to ultrasonic washing; the washing detergent is preferably water or ethanol; the water is preferably ultrapure water; the number of ultrasonic washings is preferably 2 to 3 times, more preferably 2 times; the ultrasonic time is preferably 10 to 15 min, more preferably 10 min.

[0042] After obtaining the hydrothermal precursor, the present invention places the hydrothermal precursor in a muffle furnace for calcination activation to obtain a trimetallic supported layered nanosheet electrocatalyst. The carbonization temperature is 150-300 °C, preferably 200-300 °C, more preferably 300 °C, and the holding time is preferably 0.5-4 h, more preferably 1-3 h, and further preferably 2 h; the carbonization is preferably one-step carbonization; the heating rate is preferably 5-10 °C / min, more preferably 5-8 °C / min, and further preferably 5 °C / min; the present invention exposes more active sites of the catalyst through calcination activation, and the metal inorganic part is converted into oxide / hydroxide.

[0043] The present invention also provides the use of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst described in the above scheme to electrocatalytically oxidize HMF to prepare FDCA.

[0044] In the present invention, the use of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst to electrocatalyze the oxidation of HMF to prepare FDCA preferably comprises the following steps:

[0045] The nickel-iron-cobalt trimetallic nanoarray electrocatalyst, Ag / AgCl reference electrode, graphite carbon rod counter electrode and 30 mL of electrolyte (KOH and HMF mixed solution) were placed in a 50 mL H-type electrolytic cell to form a three-electrode system for electrocatalytic oxidation reaction.

[0046] In the present invention, the electrolyte is preferably a KOH strong alkaline solution; the KOH solution concentration is preferably 10-1000 mmol / L, more preferably 1000 mmol / L; the HMF substrate concentration is preferably 10-1000 mmol / L, more preferably 20 mmol / L. The electrocatalytic oxidation applied voltage is preferably 1.0-1.8 V vs. RHE, more preferably 1.4-1.6 V vs. RHE, more preferably 1.5 V vs. RHE.

[0047] In the present invention, the KOH electrolyte and the HMF substrate are preferably mixed by ultrasonic mixing; the temperature of the electrocatalytic oxidation treatment is preferably room temperature; and the room temperature is preferably 25°C.

[0048] Specifically, the relevant preparation and detection are as follows:

[0049] Embodiment 1:

[0050] A method for electrocatalytic oxidation of 5-hydroxymethylfurfural using a nickel-iron-cobalt trimetallic nanoarray electrocatalyst comprises the following steps:

[0051] (1) Pretreatment of nickel foam: nickel foam (thickness 0.5-1.5 mm) was cut into 1-2 × 1-2 cm sizes and washed with 1 M HCl, ethanol and ultrapure water in turn to remove oxides, oil stains and residual HCl to obtain pure nickel foam;

[0052] (2) Soluble nickel salt Ni(NO3)2·6H2O, soluble iron salt Fe(NO3)3·9H2O and soluble cobalt salt Co(NO3)2·6H2O were mixed in 10 mL of ultrapure water at a molar ratio of 3:1:2, with a total amount of 0.6 mmol, and ultrasonically mixed for 10-15 min. Then, 1 mmol urea and 1 mmol NH4F were added and ultrasonically mixed to obtain a mixed solution.

[0053] (3) The pretreated pure nickel foam (0.06 g) was placed vertically into a high-pressure reactor, and the mixed solution prepared in step (2) was added. The reactor was sealed and reacted at 150 °C for 6 h. After the reactor was cooled, the nickel foam was washed with ethanol and ultrapure water in turn to obtain a layered nanosheet array precursor.

[0054] (4) The precursor obtained in step (3) is placed in a muffle furnace at 300 °C for calcination activation for 2 h, and after the reaction chamber is cooled, a nickel-iron-cobalt trimetallic nanoarray electrocatalyst is obtained.

[0055] (5) At room temperature (10-25 °C), a three-electrode system was prepared in an H-type electrolytic cell using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as the working electrode, the Ag / AgCl electrode as the reference electrode, the graphite carbon rod as the counter electrode, and a 1 M KOH solution as the electrolyte. 20 mM 5-hydroxymethylfurfural was dissolved in the electrolyte, and an electrochemical catalytic oxidation reaction was carried out for 6 h with an external voltage of 1.5 V vs. RHE on the three-electrode system.

[0056] Example 2

[0057] A method for electrocatalytic oxidation of 5-hydroxymethylfurfural using a nickel-iron-cobalt trimetallic nanoarray electrocatalyst comprises the following steps:

[0058] (1) Pretreatment of nickel foam: nickel foam (thickness 0.5-1.5 mm) was cut into 1-2 × 1-2 cm sizes and washed with 1 M HCl, ethanol and ultrapure water in turn to remove oxides, oil stains and residual HCl to obtain pure nickel foam;

[0059] (2) Soluble nickel salt Ni(NO3)2·6H2O, soluble iron salt Fe(NO3)3·9H2O and soluble cobalt salt Co(NO3)2·6H2O were mixed in 10 mL of ultrapure water at a molar ratio of 1:1:1, with a total amount of 0.6 mmol, and ultrasonically mixed for 10-15 min. Then, 1 mmol urea and 1 mmol NH4F were added and ultrasonically mixed to obtain a mixed solution.

[0060] (3) The pretreated pure nickel foam (0.06 g) was placed vertically into a high-pressure reactor, and the mixed solution prepared in step (2) was added. The reactor was sealed and reacted at 150 °C for 6 h. After the reactor was cooled, the nickel foam was washed with ethanol and ultrapure water in turn to obtain a layered nanosheet array precursor.

[0061] (4) The precursor obtained in step (3) is placed in a muffle furnace at 300 °C for calcination activation for 2 h, and after the reaction chamber is cooled, a nickel-iron-cobalt trimetallic nanoarray electrocatalyst is obtained.

[0062] (5) At room temperature (10-25 °C), a three-electrode system was prepared in an H-type electrolytic cell using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as the working electrode, the Ag / AgCl electrode as the reference electrode, the graphite carbon rod as the counter electrode, and a 1 M KOH solution as the electrolyte. 20 mM 5-hydroxymethylfurfural was dissolved in the electrolyte, and an electrochemical catalytic oxidation reaction was carried out for 6 h with an external voltage of 1.5 V vs. RHE on the three-electrode system.

[0063] Example 3

[0064] A method for electrocatalytic oxidation of 5-hydroxymethylfurfural using a nickel-iron-cobalt trimetallic nanoarray electrocatalyst comprises the following steps:

[0065] (1) Pretreatment of nickel foam: nickel foam (thickness 0.5-1.5 mm) was cut into 1-2 × 1-2 cm sizes and washed with 1 M HCl, ethanol and ultrapure water in turn to remove oxides, oil stains and residual HCl to obtain pure nickel foam;

[0066] (2) Soluble nickel salt, soluble iron salt and soluble cobalt salt Ni(NO3)2·6H2O, Fe(NO3)3·9H2O, Co(NO3)2·6H2O were mixed in 10 mL of ultrapure water at a molar ratio of 4:1:1 with a total amount of 0.6 mmol under ultrasonication for 10-15 min. Then, 1 mmol urea and 1 mmol NH4F were added and mixed under ultrasonication to obtain a mixed solution.

[0067] (3) The pretreated pure nickel foam (0.06 g) was placed vertically into a high-pressure reactor, and the mixed solution prepared in step (2) was added. The reactor was sealed and reacted at 150 °C for 6 h. After the reactor was cooled, the nickel foam was washed with ethanol and ultrapure water in turn to obtain a layered nanosheet array precursor.

[0068] (4) The precursor obtained in step (3) is placed in a muffle furnace at 300 °C for calcination activation for 2 h, and after the reaction chamber is cooled, a nickel-iron-cobalt trimetallic nanoarray electrocatalyst is obtained.

[0069] (5) At room temperature (10-25 °C), a three-electrode system was prepared in an H-type electrolytic cell using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as the working electrode, the Ag / AgCl electrode as the reference electrode, the graphite carbon rod as the counter electrode, and a 1 M KOH solution as the electrolyte. 20 mM 5-hydroxymethylfurfural was dissolved in the electrolyte, and an electrochemical catalytic oxidation reaction was carried out for 6 h with an external voltage of 1.5 V vs. RHE on the three-electrode system.

[0070] Comparative Example 1

[0071] A raw nickel foam (NF) electrocatalyst is prepared by the same method as in Example 1, except that in step 2, Ni(NO3)2·6H2O, Fe(NO3)3·9H2O and Co(NO3)2·6H2O are not added.

[0072] Comparative Example 2

[0073] A NiFe bimetallic nanoarray electrocatalyst is prepared by the same method as in Example 1, except that in step 2, Co(NO3)2·6H2O is not added, and the molar ratio of Ni(NO3)2·6H2O to Fe(NO3)3·9H2O is 3:1.

[0074] Comparative Example 3

[0075] A NiCo bimetallic nanoarray electrocatalyst is prepared by the same method as in Example 1, except that in step (2), Fe(NO3)3·9H2O is not added, and the molar ratio of Ni(NO3)2·6H2O to Co(NO3)2·6H2O is 3:2.

[0076] Comparative Examples 4 to 10

[0077] A NiFeCo tri-metallic nanoarray electrocatalyst, prepared by the same method as in Example 1, except that in step (5), the concentration of KOH electrolyte is changed to 10, 20, 50, 100, 200, 500, and 1000 mM, respectively.

[0078] Comparative Examples 11-17

[0079] A NiFeCo tri-metallic nanoarray electrocatalyst is prepared by the same method as in Example 1, except that the HMF concentration in step (5) is changed to 10, 20, 50, 100, 200, 500, and 1000 mM, respectively.

[0080] The nickel-iron-cobalt trimetallic nanoarray electrocatalyst of Example 1 of the present invention was tested using a scanning electron microscope. The results are as follows: Figure 1 , Figure 2 As shown. Figure 1 It can be seen that the catalyst prepared by the present invention maintains a good nanosheet structure, and the components are evenly distributed without obvious structural defects. Figure 2 As shown, TEM images further prove that the catalyst has a wrinkled nanosheet structure.

[0081] The nickel-iron-cobalt trimetallic nanoarray electrocatalyst of Example 1 of the present invention was subjected to an LSV scanning test, and the LSV curve is as follows: Figure 3 As shown, the catalyst of Example 1 of the present invention has a current density of 10 mA cm -2The starting potential at 20 mM HMF was only 1.26 V vs. RHE. Compared with the electrolyte without 20 mM HMF, the catalyst in the electrolyte containing 20 mM HMF showed a higher current density and a lower starting potential, indicating that the catalyst has the performance of preferentially oxidizing HMF. Example 1 was subjected to 5 consecutive electrolysis reactions. Figure 5 As shown, the nickel-iron-cobalt trimetallic nanoarray electrocatalyst can still maintain 99.7~100% HMF conversion, 97.3~98.7% FDCA yield, and 96.8~98% FE after 5 cycles.

[0082] At the same time, it can be seen from Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 in Table 1 that there is a synergistic effect between Co(NO3)2·6H2O and Fe(NO3)2·9H2O in the present invention, which can synergistically improve the relevant performance of the prepared nickel-iron-cobalt trimetallic nanoarray electrocatalyst.

[0083]

[0084] In Examples 1 to 3, the molar ratio of the nickel-iron-cobalt salt of Example 1 is moderate, so that the content of nickel-iron-cobalt ions in the obtained trimetallic catalyst is moderate, the ability of nickel ions to generate NiOOH is strong, and the generation rate is high, so it has excellent catalytic oxidation performance. When used for catalytic oxidation of HMF, the starting potential of the catalytic oxidation reaction is only 1.26 V vs. RHE, the HMF conversion rate is 100%, and the FDCA yield reaches 98.7%. Due to the low molar ratio of Example 2, the low nickel content leads to a low generation rate of NiOOH at the active site, and its overpotential and current density are both low. Because of its large molar ratio, Example 3 has a weaker metal synergy, low oxygen vacancies and iron-cobalt metal coordination sites, and poor catalytic performance.

[0085] The performance of Example 1 was compared with that of Comparative Examples 1 to 3. As shown in Table 1, Example 1 doped with iron and cobalt salts achieved a power of 10 mA cm -2 The starting potential at the current density is only 1.26 V vs. RHE, which is better than that of Comparative Examples 2 and 3. Figure 4 and Figure 5 It can be seen that Example 1 has higher HMF conversion rate (100%), FDCA yield (98.7%) and Faraday efficiency (98%). At the same time, the prepared catalyst has excellent stability and can maintain excellent electrocatalytic oxidation performance after 5 consecutive electrolysis, with HMF conversion rate of 99.7~100%, FDCA yield of 97.3~98.7% and Faraday efficiency of 96.8~98%.

[0086] At the same time, by comparing Example 1, Comparative Example 2 and Comparative Example 3, it can also be seen that there is a synergistic effect between Co(NO3)2·6H2O and Fe(NO3)3·9H2O in the present invention, which can synergistically improve the relevant performance of the prepared catalyst.

[0087] For Comparative Examples 4 to 10, the HMF concentration in the electrolyte was fixed at 20 mM, and the KOH concentration was changed to 10, 20, 50, 100, 200, 500, and 1000 mM. From the CV spectra ( Figure 6 )It can be seen that the current density increases with C OH - The current density increases with the increase of KOH concentration, and no oxidation peak appears when the KOH concentration is too low, indicating that the electrocatalytic oxidation of HMF to produce FDCA is more favorable in a strong alkaline environment and its current density depends on the KOH concentration, among which 1 M KOH has the best catalytic effect, thus verifying that the reaction belongs to the LH adsorption mechanism.

[0088] In Comparative Examples 11 to 17, the concentration of 1 M KOH in the electrolyte was fixed and the concentration of HMF was changed to 10, 20, 50, 100, 200, 500, and 1000 mM. Figure 7 ) It can be seen that as C HMF The current density increases first and then decreases, which indicates that the current density depends on the concentration of the substrate, thus further proving that the reaction belongs to the LH adsorption mechanism. The oxidation peak disappears under high concentrations of HMF, which may be attributed to the excessively fast reaction rate and the Ni 3+ Rapidly transform into Ni 2+ , which could not be detected. At the same time, we found that the catalytic effect was better when the HMF concentration was 20~50 mM.

[0089] It can be seen from the above embodiments and comparative examples that the hydrothermal pretreatment of the metal-supported layered nanosheet catalyst provided by the present invention has a low starting potential, a large current density, and excellent stability and durability, and can efficiently remove electrocatalytic oxidation of HMF to prepare FDCA, which helps to solve the problem of green and environmentally friendly energy.

[0090] In addition, high performance liquid chromatography (HPLC) was used to quantitatively and qualitatively record the dynamic changes of HMF and its oxidation products. Figure 8 The concentration changes of each substance within 6 h are shown. As the reaction time increases, the intensity of HMF decreases continuously with the increase of FDCA. The conversion of HMF is 100%, the yield of FDCA is 98.7%, and the Faradaic efficiency (FE) is 98.0%, indicating that HMF has been successfully converted into FDCA, which is better than most reported electrocatalysts (Table 2).

[0091]

[0092] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A nickel-iron-cobalt trimetallic nanoarray electrocatalyst, characterized in that: The following steps are involved: (1) Pretreatment of nickel foam: nickel foam with a thickness of 0.5-1.5 mm was cut into 1-2 × 1-2 cm sizes and washed with 1 M HCl, ethanol and ultrapure water in turn to remove oxides, oil stains and residual HCl to obtain pure nickel foam; (2) Soluble nickel salt Ni(NO3)2·6H2O, soluble iron salt Fe(NO3)3·9H2O and soluble cobalt salt Co(NO3)2·6H2O were mixed in 10 mL ultrapure water at a molar ratio of 3:1:2, with a total amount of 0.6 mmol, and ultrasonically mixed for 10-15 min. Then, 1 mmol urea and 1 mmol NH4F were added and ultrasonically mixed to obtain a mixed solution. (3) 0.06 g of pure nickel foam after pretreatment was placed vertically in a high-pressure reactor, and the mixed solution prepared in step (2) was added, and the reaction was sealed at 150 ° C for 6 h. After the reactor was cooled, the nickel foam was washed with ethanol and ultrapure water in turn to obtain a layered nanosheet array precursor; (4) The precursor obtained in step (3) is placed in a muffle furnace at 300 °C for calcination activation for 2 h, and after the reaction chamber is cooled, a nickel-iron-cobalt trimetallic nanoarray electrocatalyst is obtained.

2. Use of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as claimed in claim 1 in the electrocatalytic oxidation of 5-hydroxymethylfurfural.

3. Use of the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as claimed in claim 1 in the oxidation of 5-hydroxymethylfurfural to prepare 2,5-furandicarboxylic acid.

4. A method for electrocatalytically oxidizing 5-hydroxymethylfurfural using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as claimed in claim 1, characterized in that: The steps include: At room temperature of 10-25°C, a three-electrode system was prepared in an H-type electrolytic cell using the nickel-iron-cobalt trimetallic nanoarray electrocatalyst as a working electrode, an Ag / AgCl electrode as a reference electrode, a graphite carbon rod as a counter electrode, and a 1 M KOH solution as an electrolyte; 20 mM 5-hydroxymethylfurfural was dissolved in the electrolyte, and an electrochemical catalytic oxidation reaction was performed for 6 h by applying a voltage of 1.5 V vs. RHE to the three-electrode system; In 1.0 M KOH solution, when the current density is 10 mA cm -2 The initial potential was only 1.26 V vs. RHE; the conversion of HMF was 99.7~100% after 5 consecutive cycles, the yield of FDCA was 97.3~98.7%, and the Faradaic efficiency was 96.8~98.5%.

Citation Information

Cited By

  • Dual oxygen-containing anion co-modified nickel-based catalyst as well as preparation method and application thereof

    CN121250439A