Preparation method and application of lyocell fiber containing chlorella component

By combining Chlorella ingredients with modified melamine and modified amino silicone oil, Lycel fibers with excellent flame retardant and antibacterial properties are prepared, solving the problems of flammability and perishability of existing fibers and achieving a wider range of Applications and higher performance requirements.

CN118497918BActive Publication Date: 2024-11-15EAST CHINA UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962552.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-15
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The flame retardant and antibacterial properties of existing lyesel fibers are insufficient, which limits their application in production and life, and natural fibers are flammable and prone to rot.

Method used

The Chlorella ingredients are combined with modified melamine, modified amino silicone oil and other materials to prepare Lycel fibers with excellent flame retardant and antibacterial properties through modified spinning technology. The method includes reacting tetrahydroxymethylphosphate with melamine to form modified melamine, adding 1,2-epoxypropyldimethyldodecyl ammonium chloride for grafting, followed by adding sodium metaaluminate and aluminum sulfate Flame-retardant antibacterial compounds are formed and combined with modified amino silicone oil and Chlorella extract to prepare high-performance fibers through spinning process.

Benefits of technology

It significantly improves the flame retardant and antibacterial properties of the fiber, making it more flexible, breathable, and has antistatic and antifouling properties. It is suitable for the production of inner linings of facial masks, masks, fireproof clothing and heat-insulating clothing, expanding the application field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of lyocell fibers, and discloses a method for preparing lyocell fibers containing chlorella components and applications thereof, which are prepared by modified spinning of lyocell fiber raw materials, flame retardant and antibacterial compounds, modified amino silicone oils, and chlorella extracts. The flame retardant and antibacterial compounds are prepared by modifying melamine with tetrakis hydroxymethylphosphonium sulfate, grafting 1,2-epoxypropyldimethyldodecylammonium chloride, and adding sodium aluminate and aluminum sulfate. The modified amino silicone oil is modified with epoxy polyether and grafted with quinoline-6-carboxylic acid. The lyocell fibers of the invention have excellent flame retardant and antibacterial properties, and the modified silicone oil is added to make the fibers smoother and more compliant, and can be used for the production of linings of facial masks, masks, fireproof clothing, and heat-insulating clothing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lyocell fibers, in particular to a preparation method and application of lyocell fibers containing chlorella components. Background Art

[0002] Lyocell fiber, commonly known as "Tencel", has the excellent properties of both natural and synthetic fibers. It is a truly green fiber that comes from cellulose in nature and has a non-toxic and harmless production process. Lyocell fiber has the characteristics of comfort, good hand feel, and easy dyeing. Compared with viscose fiber, the production process is more environmentally friendly. Lyocell fiber is closer to natural fiber, which is flammable and unsafe in production and life. At the same time, natural fiber is also the most prone to corruption. Therefore, improving the flame retardant and antibacterial properties of Lyocell fiber will greatly help expand the application of Lyocell fiber. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of lyocell fiber containing chlorella ingredients, which has excellent antibacterial and flame retardant properties and is smoother.

[0005] (II) Technical solution

[0006] A method for preparing lyocell fiber containing chlorella ingredients is as follows:

[0007] (1) Tetrakis (hydroxymethyl) phosphonium sulfate is added to deionized water, and melamine is added under stirring, and the temperature is raised to 90-110°C, and the reaction is carried out for 3-8 hours. After cooling, the mixture is filtered, washed with deionized water for 3-6 times, and dried to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine;

[0008] (2) adding tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into sodium hydroxide solution, stirring evenly, adding 1,2-epoxypropyldimethyldodecylammonium chloride, stirring and heating to 90-120°C, reacting for 2-6 hours, cooling to room temperature, and obtaining a melamine modified grafted product;

[0009] (3) adding sodium aluminate and aluminum sulfate to the melamine-modified grafted product and ultrasonically dispersing the product for 5 to 20 minutes to obtain a flame retardant and antibacterial compound;

[0010] (4) a,ω-dihydroxypolydimethylsiloxane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and potassium hydroxide are mixed, nitrogen is passed through, and the mixture is reacted at 80-100°C for 5-10 h. Epoxy polyether is added thereto, and the mixture is reacted at 70-90°C for 2-10 h. The solvent is removed under reduced pressure. Quinoline-6-carboxylic acid is added to water to prepare a solution, and a catalyst, a strongly acidic ion exchange resin, is added thereto, and the mixture is heated under reflux for 10-20 h to obtain a modified amino silicone oil.

[0011] (5) placing the Chlorella in a dialysis bag and centrifuging, combining the supernatant, extracting with ethyl acetate, separating, and evaporating and concentrating the ethyl acetate extract to obtain a Chlorella extract;

[0012] (6) Adding lyocell fiber raw materials into an N-methylmorpholine aqueous solution, stirring to dissolve, adding flame retardant and antibacterial compounds, modified amino silicone oil and cross-linking agent terephthalic acid, heating and vacuum distilling to obtain a spinning solution, adding chlorella extract, stirring evenly, spinning, oiling, and drying to obtain lyocell fiber.

[0013] Preferably, in step (1), the mass ratio of tetrakis(hydroxymethyl)phosphonium sulfate to melamine is 1:1.5-3.

[0014] Preferably, in step (2), the mass ratio of tetrakis(hydroxymethyl)phosphonium sulfate-modified melamine to 1,2-epoxypropyldimethyldodecylammonium chloride is 1:0.3-0.6.

[0015] Preferably, in step (3), the mass ratio of the melamine-modified grafted product, sodium aluminate and aluminum sulfate is 1:0.2-0.6:0.2-0.6.

[0016] Preferably, in step (4), the mass ratio of a,ω-dihydroxypolydimethylsiloxane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, potassium hydroxide, epoxy polyether, and quinoline-6-carboxylic acid is 1:0.2~0.6:0.01~0.05:0.2~0.4:0.3~0.6.

[0017] Preferably, in step (6), the mass ratio of the lyocell fiber raw material, the flame retardant and antibacterial compound, the modified amino silicone oil, terephthalic acid, and the Chlorella extract is 1:0.1~0.3:0.1~0.3:0.01~0.03:0.1~0.3.

[0018] Preferably, the lyocell fiber raw material in step (6) is hemp pulp, straw pulp, cotton pulp, wood pulp or bamboo pulp.

[0019] Preferably, the lyocell fiber containing chlorella components is used in the production of linings for facial masks, masks, fireproof clothing and heat-insulating clothing.

[0020] 3. Beneficial technical effects

[0021] A lyocell fiber containing chlorella is prepared by modified spinning of lyocell fiber raw material, flame retardant and antibacterial compound, modified amino silicone oil and chlorella extract. The flame retardant and antibacterial compound is prepared by modifying melamine with tetrakis hydroxymethyl phosphonium sulfate and grafting 1,2-epoxypropyl dimethyl dodecyl ammonium chloride. The modified amino silicone oil is prepared by modifying epoxy polyether and grafting quinoline-6-carboxylic acid.

[0022] Compared with the existing technology: the flame retardant and antibacterial components are synthesized into a new type of component, which is more convenient to produce and use, has both flame retardant and antibacterial effects, and has a wider range of applications. Modified amino silicone oil can improve the quality of fibers, making them more supple and hygroscopic. The resulting textiles have better air permeability and have certain antistatic and antifouling properties. The chlorella component greatly improves the skin-friendliness of woven textiles, making them more supple.

[0023] The lyocell fiber of the present invention has excellent flame retardant and antibacterial properties, and the addition of modified silicone oil makes the fiber smoother and more flexible, and can be used for the production of linings of facial masks, masks, fireproof clothing and heat-insulating clothing. DETAILED DESCRIPTION

[0024] Example 1

[0025] (1) Add 10 g of tetrakis (hydroxymethyl) phosphonium sulfate to deionized water, add 15 g of melamine under stirring, heat to 90°C, react for 3 h, cool and filter, wash with deionized water 3 times, and dry to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine.

[0026] (2) Add 20 g of tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into a sodium hydroxide solution, stir evenly, add 6 g of 1,2-epoxypropyldimethyldodecylammonium chloride, stir and heat to 90°C, react for 2 h, and cool to room temperature to obtain tetrakis(hydroxymethyl)phosphonium sulfate modified melamine grafted with 1,2-epoxypropyldimethyldodecylammonium chloride, i.e., melamine modified grafted product.

[0027] (3) Add 4 g of sodium aluminate and 4 g of aluminum sulfate to 20 g of the melamine-modified grafted product and disperse them ultrasonically for 5 min to obtain a flame retardant and antibacterial compound.

[0028] (4) 30 g of ω-dihydroxypolydimethylsiloxane, 6 g of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, and 0.3 g of potassium hydroxide were mixed, nitrogen was passed through, and the mixture was reacted at 80°C for 5 h. 6 g of epoxy polyether was added thereto, and the mixture was reacted at 70°C for 2 h. The solvent was removed under reduced pressure. 9 g of quinoline-6-carboxylic acid was added to 50 mL of water to prepare a solution, and 6 g of a catalyst, a strongly acidic ion exchange resin, was added thereto. The mixture was heated under reflux for 10 h to obtain a modified amino silicone oil.

[0029] (5) Place the Chlorella in a dialysis bag and centrifuge, combine the supernatant, extract with ethyl acetate, separate, and evaporate and concentrate the ethyl acetate extract to obtain the Chlorella extract.

[0030] (6) Add 80 g of lyocell fiber raw material into 400 mL of N-methylmorpholine aqueous solution and stir to dissolve. Add 8 g of flame retardant and antibacterial compound, 8 g of modified amino silicone oil and 0.8 g of cross-linking agent terephthalic acid. Heat and distill under negative pressure to obtain a spinning solution. Add 8 g of Chlorella extract and stir evenly. Spin, oil and dry to obtain Lyocell fiber.

[0031] Example 2

[0032] (1) Add 30 g of tetrakis (hydroxymethyl) phosphonium sulfate to deionized water, add 90 g of melamine under stirring, heat to 110°C, react for 8 h, cool and filter, wash with deionized water 6 times, and dry to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine.

[0033] (2) Add 60 g of tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into sodium hydroxide solution, stir evenly, add 36 g of 1,2-epoxypropyldimethyldodecylammonium chloride, stir and heat to 120°C, react for 6 h, and cool to room temperature to obtain tetrakis(hydroxymethyl)phosphonium sulfate modified melamine grafted with 1,2-epoxypropyldimethyldodecylammonium chloride, i.e., melamine modified graft product.

[0034] (3) Add 40 g of sodium aluminate and 40 g of aluminum sulfate to 70 g of the melamine-modified grafted product and disperse them ultrasonically for 20 min to obtain a flame retardant and antibacterial compound.

[0035] (4) 60 g of ω-dihydroxypolydimethylsiloxane, 36 g of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and 3 g of potassium hydroxide were mixed, nitrogen was passed through, and the mixture was reacted at 100 °C for 10 h. 24 g of epoxy polyether was added thereto, and the mixture was reacted at 90 °C for 10 h. The solvent was removed under reduced pressure. 36 g of quinoline-6-carboxylic acid was added to 200 mL of water to prepare a solution, and 15 g of a catalyst strong acid ion exchange resin was added thereto. The mixture was heated under reflux for 20 h to obtain a modified amino silicone oil.

[0036] (5) Place the Chlorella in a dialysis bag and centrifuge, combine the supernatant, extract with ethyl acetate, separate, and evaporate and concentrate the ethyl acetate extract to obtain the Chlorella extract.

[0037] (6) Add 120 g of lyocell fiber raw material into 800 mL of N-methylmorpholine aqueous solution and stir to dissolve. Add 36 g of flame retardant and antibacterial compound, 36 g of modified amino silicone oil and 3.6 g of cross-linking agent terephthalic acid. Heat and distill under negative pressure to obtain a spinning solution. Add 36 g of Chlorella extract and stir evenly. Spin, oil and dry to obtain Lyocell fiber.

[0038] Example 3

[0039] (1) Add 15 g of tetrakis (hydroxymethyl) phosphonium sulfate to deionized water, add 30 g of melamine under stirring, heat to 100 °C, react for 5 h, cool and filter, wash with deionized water 4 times, and dry to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine.

[0040] (2) Add 30 g of tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into a sodium hydroxide solution, stir evenly, add 10 g of 1,2-epoxypropyldimethyldodecylammonium chloride, stir and heat to 100°C, react for 3 h, and cool to room temperature to obtain tetrakis(hydroxymethyl)phosphonium sulfate modified melamine grafted with 1,2-epoxypropyldimethyldodecylammonium chloride, i.e., melamine modified grafted product.

[0041] (3) Add 10 g of sodium aluminate and 10 g of aluminum sulfate to 30 g of the melamine-modified grafted product and disperse them ultrasonically for 15 min to obtain a flame retardant and antibacterial compound.

[0042] (4) 40 g of ω-dihydroxypolydimethylsiloxane, 10 g of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and 1 g of potassium hydroxide were mixed, nitrogen was passed through, and the mixture was reacted at 90 °C for 6 h. 10 g of epoxy polyether was added thereto, and the mixture was reacted at 80 °C for 4 h. The solvent was removed under reduced pressure. 15 g of quinoline-6-carboxylic acid was added to 100 mL of water to prepare a solution, and 10 g of a catalyst, a strongly acidic ion exchange resin, was added thereto. The mixture was heated under reflux for 12 h to obtain a modified amino silicone oil.

[0043] (5) Place the Chlorella in a dialysis bag and centrifuge, combine the supernatant, extract with ethyl acetate, separate, and evaporate and concentrate the ethyl acetate extract to obtain the Chlorella extract.

[0044] (6) Add 90 g of lyocell fiber raw material into 500 mL of N-methylmorpholine aqueous solution and stir to dissolve. Add 10 g of flame retardant and antibacterial compound, 10 g of modified amino silicone oil and 1 g of cross-linking agent terephthalic acid. Heat and distill under negative pressure to obtain a spinning solution. Add 10 g of Chlorella extract and stir evenly. Spin, oil and dry to obtain Lyocell fiber.

[0045] Example 4

[0046] (1) Add 20 g of tetrakis (hydroxymethyl) phosphonium sulfate to deionized water, add 50 g of melamine under stirring, heat to 100 °C, react for 6 h, cool and filter, wash with deionized water 5 times, and dry to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine.

[0047] (2) Add 40 g of tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into a sodium hydroxide solution, stir evenly, add 20 g of 1,2-epoxypropyldimethyldodecylammonium chloride, stir and heat to 120°C, react for 5 h, and cool to room temperature to obtain tetrakis(hydroxymethyl)phosphonium sulfate modified melamine grafted with 1,2-epoxypropyldimethyldodecylammonium chloride, i.e., melamine modified grafted product.

[0048] (3) Add 20 g of sodium aluminate and 20 g of aluminum sulfate to 40 g of melamine-modified grafted product and disperse them ultrasonically for 10 min to obtain a flame retardant and antibacterial compound.

[0049] (4) 50 g of ω-dihydroxypolydimethylsiloxane, 20 g of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and 2 g of potassium hydroxide were mixed, nitrogen was passed through, and the mixture was reacted at 100 °C for 10 h. 15 g of epoxy polyether was added thereto, and the mixture was reacted at 80 °C for 6 h. The solvent was removed under reduced pressure. 20 g of quinoline-6-carboxylic acid was added to 150 mL of water to prepare a solution, and 10 g of a catalyst strong acid ion exchange resin was added thereto. The mixture was heated under reflux for 16 h to obtain a modified amino silicone oil.

[0050] (5) Place the Chlorella in a dialysis bag and centrifuge, combine the supernatant, extract with ethyl acetate, separate, and evaporate and concentrate the ethyl acetate extract to obtain the Chlorella extract.

[0051] (6) Add 110 g of lyocell fiber raw material into 600 mL of N-methylmorpholine aqueous solution and stir to dissolve. Add 20 g of flame retardant and antibacterial compound, 20 g of modified amino silicone oil and 2 g of cross-linking agent terephthalic acid. Heat and distill under negative pressure to obtain a spinning solution. Add 20 g of Chlorella extract and stir evenly. Spin, oil and dry to obtain Lyocell fiber.

[0052] Example 5

[0053] (1) Add 30 g of tetrakis (hydroxymethyl) phosphonium sulfate to deionized water, add 80 g of melamine under stirring, heat to 110°C, react for 6 h, cool and filter, wash with deionized water 5 times, and dry to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine.

[0054] (2) Add 50 g of tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into a sodium hydroxide solution, stir evenly, add 30 g of 1,2-epoxypropyldimethyldodecylammonium chloride, stir and heat to 120°C, react for 2 h, and cool to room temperature to obtain tetrakis(hydroxymethyl)phosphonium sulfate modified melamine grafted with 1,2-epoxypropyldimethyldodecylammonium chloride, i.e., melamine modified graft product.

[0055] (3) Add 30 g of sodium aluminate and 30 g of aluminum sulfate to 60 g of melamine-modified grafted product and disperse them by ultrasonic for 20 min to obtain a flame retardant and antibacterial compound.

[0056] (4) 45 g of ω-dihydroxypolydimethylsiloxane, 20 g of N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and 2 g of potassium hydroxide were mixed, nitrogen was passed through, and the mixture was reacted at 100 °C for 10 h. 15 g of epoxy polyether was added thereto, and the mixture was reacted at 90 °C for 5 h. The solvent was removed under reduced pressure. 25 g of quinoline-6-carboxylic acid was added to 180 mL of water to prepare a solution, and 12 g of a catalyst strong acid ion exchange resin was added thereto. The mixture was heated under reflux for 18 h to obtain a modified amino silicone oil.

[0057] (5) Place the Chlorella in a dialysis bag and centrifuge, combine the supernatant, extract with ethyl acetate, separate, and evaporate and concentrate the ethyl acetate extract to obtain the Chlorella extract.

[0058] (6) Add 100 g of lyocell fiber raw material into 800 mL of N-methylmorpholine aqueous solution and stir to dissolve. Add 30 g of flame retardant and antibacterial compound, 30 g of modified amino silicone oil and 3 g of cross-linking agent terephthalic acid. Heat and distill under negative pressure to obtain a spinning solution. Add 30 g of Chlorella extract and stir evenly. Spin, oil and dry to obtain Lyocell fiber.

[0059] Comparative Example 1: Ordinary lyocell fiber.

[0060] Comparative Example 2: Chlorella extract was added to ordinary lyocell fiber, and the preparation process was the same as that of Example 1.

[0061] Performance Testing:

[0062] The fibers of Examples 1 to 5 and Comparative Examples 1 to 2 were put into a weaving machine for weaving into samples of 300 mm×89 mm, and then tested.

[0063] 1. The combustion performance of Examples 1 to 5 and Comparative Example 1 was tested according to the method of GB / T 5455-2014. The results are shown in Table 1. 2. Antibacterial performance test of Staphylococcus aureus: The cultured Staphylococcus aureus slant was scraped with sterile saline and the bacteria were fully shaken to disperse. A nutrient agar medium (4 g agar / 50 mL H 2 O) Place on an electric stove to dissolve and sterilize, and after cooling slightly (40°C), mix the pre-prepared Staphylococcus aureus suspension according to the aseptic operation requirements and shake it thoroughly, then immediately pour it into a sterile culture dish (about 15 mL per dish), rotate it quickly, and then let it stand horizontally to condense (the surface must be smooth and flat, and the thickness must be uniform). The textiles prepared in Examples 1 to 5 and Comparative Example 1 are crushed, 1 g of the powder sample is taken, and a glass ring (with an inner diameter of 1.8 cm) is gently placed in the center of the plate in the culture dish with tweezers, and gently compacted to prevent the powder from squeezing out from the bottom when compacting, and then the powder sample is added to the glass ring through the feeding funnel, and is stirred and compacted with a glass rod (preferably without damaging the agar plate). Cover the dish with a lid and place it in a bacterial incubator at 37°C for 24 h. Measure the size of the inhibition zone. The results are shown in Table 2. 3. Test the sustained-release performance: The fibers of Examples 1 to 5 and Comparative Example 2 were made into mask base fabrics using a FZS-600 nonwoven material carding machine and a FZZ-1000 needle punching machine (Changshu Weicheng Nonwoven Equipment Co., Ltd.). 5 g of the mask base fabric was placed in a 1000 mL beaker, and 400 mL of deionized water was added. The fabrics were soaked for 2, 4, 6, 8, 10, 12, 14, and 16 min, respectively. The extracts were collected, concentrated by rotary evaporation, and the content of the active ingredient, Chlorella polysaccharides, was determined by liquid chromatography. The results are shown in Table 3.

[0064] Table 1: GB / T 5455-2014 Combustion performance test data

[0065]

[0066] Table 2: Antibacterial performance test

[0067]

[0068] Table 3 Test results

[0069]

[0070] It can be seen from Tables 1, 2 and 3 that the flame retardant and antibacterial properties of Examples 1 to 5 are better than those of Comparative Example 1. The facial masks prepared from the lyocell fibers of Examples 1 to 5 have better sustained-release properties and are better used in the facial mask industry.

[0071] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing lyocell fiber containing chlorella, characterized in that: The preparation method is as follows: (1) Tetrakis (hydroxymethyl) phosphonium sulfate is added to deionized water, and melamine is added under stirring, and the temperature is raised to 90-110°C, and the reaction is carried out for 3-8 hours. After cooling, the mixture is filtered, washed with deionized water for 3-6 times, and dried to obtain tetrakis (hydroxymethyl) phosphonium sulfate-modified melamine; (2) adding tetrakis(hydroxymethyl)phosphonium sulfate modified melamine into sodium hydroxide solution, stirring evenly, adding 1,2-epoxypropyldimethyldodecylammonium chloride, stirring and heating to 90-120°C, reacting for 2-6 hours, cooling to room temperature, and obtaining a melamine modified grafted product; (3) adding sodium aluminate and aluminum sulfate to the melamine-modified grafted product and ultrasonically dispersing the product for 5 to 20 minutes to obtain a flame retardant and antibacterial compound; (4) a,ω-dihydroxypolydimethylsiloxane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane and potassium hydroxide are mixed, nitrogen is passed through, and the mixture is reacted at 80-100°C for 5-10 h, epoxy polyether is added thereto, and the mixture is reacted at 70-90°C for 2-10 h, the solvent is removed under reduced pressure, quinoline-6-carboxylic acid is added to water to prepare a solution, a catalyst strong acid ion exchange resin is added, and the mixture is heated under reflux for 10-20 h to obtain a modified amino silicone oil; (5) placing the Chlorella in a dialysis bag and centrifuging, combining the supernatant, extracting with ethyl acetate, separating, and evaporating and concentrating the ethyl acetate extract to obtain a Chlorella extract; (6) Adding lyocell fiber raw materials into an N-methylmorpholine aqueous solution, stirring to dissolve, adding flame retardant and antibacterial compounds, modified amino silicone oil and cross-linking agent terephthalic acid, heating and vacuum distilling to obtain a spinning solution, adding chlorella extract, stirring evenly, spinning, oiling, and drying to obtain lyocell fiber.

2. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (1), the mass ratio of tetrakis(hydroxymethyl)phosphonium sulfate to melamine is 1:1.5-3.

3. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (2), the mass ratio of tetrakis(hydroxymethyl)phosphonium sulfate-modified melamine to 1,2-epoxypropyldimethyldodecylammonium chloride is 1:0.3-0.

6.

4. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (3), the mass ratio of the melamine-modified grafted product, sodium aluminate and aluminum sulfate is 1:0.2-0.6:0.2-0.

6.

5. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (4), the mass ratio of a,ω-dihydroxypolydimethylsiloxane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, potassium hydroxide, epoxy polyether, and quinoline-6-carboxylic acid is 1:0.2~0.6:0.01~0.05:0.2~0.4:0.3~0.

6.

6. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (6), the mass ratio of the lyocell fiber raw material, the flame retardant and antibacterial compound, the modified amino silicone oil, terephthalic acid, and the Chlorella extract is 1:0.1-0.3:0.1-0.3:0.01-0.03:0.1-0.

3.

7. The method for preparing lyocell fiber containing chlorella component according to claim 1, characterized in that: In the step (6), the lyocell fiber raw material is hemp pulp, straw pulp, cotton pulp, wood pulp or bamboo pulp.

8. The use of the Lyocell fiber containing chlorella component prepared by the method for preparing Lyocell fiber containing chlorella component according to claim 1, characterized in that: The lyocell fiber containing chlorella components is used in the production of linings of facial masks, masks, fireproof clothing and heat-insulating clothing.