A protease bioreactor and its preparation method and application
By modifying polymer brushes onto magnetic nanoparticles and covalently linking them with proteases to form nanoparticles, the leakage and diffusion problems in the protease immobilization process are solved, improving the enzymatic hydrolysis efficiency and activity, and enabling simple separation of enzymatic hydrolysis products.
Patent Information
- Application Number
- CN202411026483.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The lack of effective support materials and immobilization methods in the existing technology leads to easy leakage of proteases during immobilization, slow diffusion of substrates and products, loss of enzyme activity, and difficulty in reuse.
Magnetic nanoparticles were modified with polymer brushes, and proteases were immobilized through covalent linkage to form nanoparticles of magnetic core@biocompatible layer@polymer brush-protease. The polymer brushes provided more active sites and high loading capacity, combined with the convenient separation of magnetic nanoparticles.
It improves the immobilization rate and activity of protease, increases the contact area between enzyme and substrate, simplifies the separation of products after enzymatic hydrolysis, and provides an efficient and sustainable enzyme catalytic reaction scheme.
Smart Images

Figure CN118546777B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of bioengineering, and in particular to a protease bioreactor and a preparation method and application thereof. Background Art
[0002] Proteases are hydrolases responsible for hydrolyzing peptide bonds in proteins. Proteases can be isolated from microorganisms, plants and animals and are widely used in industries such as pharmaceuticals, analysis, diagnosis and wastewater treatment. Trypsin is one of the most important protein digestive enzymes, which selectively catalyzes the hydrolysis of peptide bonds between arginine and lysine amino acid residues in proteins. Therefore, it is widely used in industry and research to hydrolyze proteins.
[0003] In recent years, trypsin has played a vital role in proteomics research. As a hydrolase, trypsin selectively hydrolyzes peptide bonds in proteins, especially at the carboxyl positions of arginine, lysine and histidine, to produce short peptide chains and amino acids, making proteins easier to analyze. Its application in mass spectrometry pretreatment helps convert complex protein samples into peptide fragments that are easy to analyze, improving the accuracy and sensitivity of the analysis. Trypsin can also be used to prepare peptide fragments, which can be analyzed by mass spectrometry for protein identification and quantification, providing key data for understanding the composition, structure and function of proteins. In addition, trypsin also plays a role in phosphorylation site identification, helping to determine phosphorylation sites by generating phosphorylated peptide fragments. However, there are some limitations to the use of free trypsin in these applications, such as difficulty in recovering from the reaction system, long reaction time, low sensitivity, low hydrolysis efficiency, and easy self-digestion, resulting in the generation of unwanted fragments and affecting reaction efficiency.
[0004] Encapsulation or immobilization of biomolecules refers to the use of solid materials to confine or bind biomolecules such as proteins, enzymes, and nucleic acids to a certain area to protect them from inactivation or denaturation due to external environmental stimulation (such as organic solvents, temperature, pH, etc.). Typical techniques for immobilizing proteases can be divided into two categories: (a) physical methods, such as adsorption, encapsulation, and embedding; and (b) chemical methods, including electrostatic interactions, fixation with metal chelation, and covalent bonding. Physical immobilization using encapsulation and embedding techniques is common, but there are some disadvantages, including enzyme leakage and slow diffusion mass transfer of substrates and products within the support matrix. Methods based on physical adsorption and electrostatic interactions are easy to implement, but are accompanied by nonspecific protein binding and the risk of losing enzymes during operation. Covalent bonding is the most effective method to prevent enzymes from falling off the support during operation. This benefit comes at the cost of denaturation and inactivation due to distortion of the three-dimensional conformation of the protein caused by multi-point binding. In addition, typical solid supports used for covalent immobilization are usually not easily regenerated after the inactivation of the immobilized enzyme.
[0005] Therefore, the development of new support materials and immobilization methods to achieve strong and reversible binding of enzymes has become an urgent goal. Summary of the invention
[0006] In response to the above-mentioned problem of lack of new supporting materials and fixation methods for covalently fixing proteases, the present invention provides a protease bioreactor, which modifies the outer shell of magnetic nanoparticles with a polymer brush, and then covalently connects the polymer brush to the protease. The resulting nanoparticles of nanomagnetic core@biocompatible layer@polymer brush-protease have excellent protease bioreactor characteristics.
[0007] On the one hand, the present invention discloses a protease bioreactor, comprising a nanomagnetic core made of a magnetic material, a biocompatible layer made of a biocompatible material, a polymer brush having an azolactone functional group and a protease, wherein the polymer brush is at least one of poly(2-vinyl-4,4-dimethyl-2-oxazolin-5-one) (pVDMA), poly(2-vinyl-4,4-dimethyl-2-morpholine-5-one), 2-vinyl-4-isopropyl-2-morpholine-5-one), poly(2-vinyl-4,4-diethyl-2-morpholine-5-one), and poly(glycidyl methacrylate) (pGMA); the biocompatible layer is coated on the outside of the nanomagnetic core, the polymer brush is grafted and modified on the biocompatible layer, the protease is covalently linked to the polymer brush, and a nanoparticle of nanomagnetic core@biocompatible layer@polymer brush-protease is formed, which is a protease bioreactor.
[0008] The inventor considers that enzyme can be reused in the immobilized enzyme technology, and protease is fixed on the magnetic nanoparticle, so that enzyme can be easily removed from the reaction mixture. Like this, they can be used under various treatment conditions. Ideally, substrate and reaction specificity and enzyme reactivity should not be lost due to immobilization. Based on the above considerations, the present invention aims to utilize magnetic nanoparticles in conjunction with the immobilized enzyme technology, protease is fixed on the magnetic nanoparticle, improves the enzymatic activity of protease, enables protease to fully hydrolyze protein, improves its application performance, and currently available fixation methods and materials are not abundant.
[0009] After a lot of preliminary research and repeated exploration, the inventors proposed that polymer brushes could be used to modify magnetic nanoparticles. By modifying the magnetic nanoparticles with polymer brushes, the polymer brushes provide many active sites on the outer shell of the magnetic nanoparticles, providing a larger surface area for enzyme immobilization, and have the advantages of high loading capacity, easy separation from the reaction mixture and reusability. A biocompatible layer is coated on the outside of the nanomagnetic core to improve compatibility with proteins, ensuring that the biological function of the protease is not affected after being connected to the polymer brush.
[0010] The protease bioreactor of the present invention can modify the silane thiol group on the surface of the nanomagnetic core@biocompatible layer particles to react the thiol group with the polymer brush monomer molecules, and utilize the surface-initiated atom transfer radical polymerization technology to in situ grow hairy polymer chains to form polymer brush modified magnetic nanoparticles, and finally obtain a protease bioreactor of nanoparticles of nanomagnetic core@biocompatible layer@polymer brush-protease, which has the advantages of high protease fixation rate, high enzyme activity and high peptide coverage after enzyme cleavage.
[0011] pVDMA, pGMA, etc. can react with the amino or thiol groups of the enzyme to form a stable connection and achieve rapid and effective immobilization. In particular, the polymer pVDMA of 2-vinyl-4,4-dimethyl-2-oxazolin-5-one (VDMA) can be used as a convenient reactive scaffold because its dimethyl azolactone ring is easily opened by nucleophiles (such as amines, hydroxyls and thiols), and easily reacts with the amino or thiol groups of the enzyme to achieve rapid and effective immobilization. Compared with other activated esters, the advantage of the azolactone functional group is that the ring-opening reaction with nucleophiles is an addition reaction to form a covalent bond. In addition, the polymer brush modified on the surface of magnetic nanoparticles can provide many binding sites and further serve as a scaffold to support three-dimensional enzyme immobilization.
[0012] In some of the embodiments, the magnetic material is Fe3O4.
[0013] In some embodiments, the biocompatible material is SiO2.
[0014] In some embodiments, the protease is trypsin.
[0015] In some of the solutions, the mass ratio of the nanomagnetic core@biocompatible layer@polymer brush to the protease is 1:0.1-1. With this ratio, the obtained protease bioreactor has better enzymolysis efficiency.
[0016] In some of the solutions, the mass ratio of the nanomagnetic core@biocompatible layer@polymer brush to the protease is 1:0.18-0.22, and further 1:0.20. With this ratio, the obtained protease bioreactor has the best enzymatic hydrolysis efficiency.
[0017] In some embodiments, the particle size of the nanomagnetic core is 10 nm-1 μm.
[0018] In some embodiments, the biocompatible layer has a thickness of 5-10 nm.
[0019] In some embodiments, the polymer brush has a thickness of 10-50 nm.
[0020] On the other hand, the present invention also discloses a method for preparing the above-mentioned protease bioreactor, wherein the nanoparticles are Fe3O4@SiO2@polymer brush-protease, comprising the following steps:
[0021] Preparation of S1, Fe3O4@SiO2 magnetic nanoparticles:
[0022] Fe3O4 nano-magnetic cores are dispersed in a solvent, and a silicon source precursor is added in an alkaline environment to react and obtain Fe3O4@SiO2 magnetic nanoparticles;
[0023] Preparation of S2, Fe3O4@SiO2@polymer brush magnetic nanoparticles:
[0024] Fe3O4@SiO2 magnetic nanoparticles are dispersed in a solvent, a thiolating agent is added to carry out a thiolating reaction, the system solvent is replaced with a non-protonic polar solvent, and then an immobilized initiator and a polymer brush monomer are added to carry out an atom transfer radical polymerization reaction to obtain Fe3O4@SiO2@polymer brush magnetic nanoparticles;
[0025] Preparation of S3, Fe3O4@SiO2@polymer brush-protease nanoparticles:
[0026] The protease is dissolved in a solvent to obtain a protease solution, and the protease solution is added into a Fe3O4@SiO2@polymer brush magnetic nanoparticle dispersion to allow the protease to react with the Fe3O4@SiO2@polymer brush magnetic nanoparticles and be fixed on the Fe3O4@SiO2@polymer brush magnetic nanoparticles.
[0027] The above preparation method first coats the surface of Fe3O4 with a highly biocompatible SiO2 layer to increase the affinity with proteases, and then uses atom transfer radical polymerization (ATRP) technology to grow polymer chains in situ on the surface of the immobilized initiator through active controlled polymerization. Compared with the "grafting to" method, the above "de novo grafting" (ATRP) technology can significantly increase the surface grafting density, and the polymer structure and thickness are well controlled. In addition, the non-cross-linked polymer chain not only provides a large number of binding sites, but also serves as a scaffold to support the three-dimensional immobilization of trypsin, thereby increasing the loading capacity and improving the accessibility of immobilized trypsin.
[0028] In some of the schemes, in step S2, the immobilized initiator is azobisisobutyronitrile.
[0029] In some of the schemes, in step S2, the aprotic polar solvent is N,N'-dimethylformamide.
[0030] In some of the schemes, in step S2, the polymer brush monomer is 2-vinyl-4,4-dimethyl-2-oxazolin-5-one (VDMA) or glycidyl methacrylate (GMA).
[0031] In some of the schemes, in step S2, the usage ratio of the Fe3O4@SiO2 magnetic nanoparticles to the polymer brush monomer is 12g:1-100mmol, preferably 12g:5-20mmol, and more preferably 12g:10mmol.
[0032] In some of the schemes, in step S2, the mass ratio of the Fe3O4@SiO2 magnetic nanoparticles to the immobilized initiator is 120:600-1000, preferably 120:700-900, and more preferably 120:800.
[0033] In some of the schemes, in step S2, the atom transfer radical polymerization reaction is carried out at 50-90°C, preferably 60-80°C, and more preferably 70°C.
[0034] In some of the schemes, in step S2, the atom transfer radical polymerization reaction time is 10-30 h, preferably 15-20 h, and more preferably 17 h.
[0035] In some of the schemes, in step S2, the solvent is ethanol.
[0036] In some of the schemes, in step S2, the thiolating agent is 3-mercaptopropyltrimethoxysilane.
[0037] In some of the schemes, in step S2, the thiolation reaction is carried out at 10-40°C, preferably 20-30°C.
[0038] In some of the schemes, in step S2, the thiolation reaction time is 8-16 h, preferably 10-14 h, and more preferably 12 h.
[0039] In-situ grafting of polymer compound brushes under the above conditions can significantly increase the surface grafting density and well control the polymer structure and thickness.
[0040] In some of the schemes, before step S1, the following step S0 is also included:
[0041] Preparation of S0, Fe3O4 nano magnetic cores: Mix a mixed solution containing an iron precursor and a reducing agent with an alkaline reagent in a solvent, heat and react to obtain the obtained product.
[0042] It is understandable that the preparation of Fe3O4 nano-magnetic cores can also be prepared according to conventional methods, but the above method has the advantage of being simple and easy to obtain.
[0043] In some of the schemes, in step S0, the temperature of the heating reaction is 190-220°C, preferably 195-205°C, and more preferably 200°C.
[0044] In some of the schemes, in step S0, the heating reaction time is 6-72 h, preferably 8-13 h, and more preferably 10 h.
[0045] In some of the schemes, in step S0, the iron precursor includes at least one of ferrous chloride, ferric acetylacetonate, ferric chloride and ferric oxide, preferably ferric chloride.
[0046] In some of the schemes, in step S0, the reducing agent is sodium citrate.
[0047] In some of the schemes, in step S0, the molar ratio of the iron precursor to the reducing agent is 2-6:1, preferably 3.5-4.5:1, more preferably 3.9-4.1:1, and most preferably 3.98:1.
[0048] In some of the schemes, in step S0, the alkaline reagent is sodium acetate and / or sodium hydroxide, preferably sodium acetate.
[0049] In some of the schemes, in step S0, the molar ratio of the iron precursor to the alkaline reagent is 1.0-2.0:1, preferably 1.1-1.4:1, more preferably 1.2-1.3:1, and most preferably 1.26:1.
[0050] In some of the schemes, in step S0, the solvent is ethylene glycol.
[0051] In some of the schemes, in step S1, before adding the silicon source precursor, ammonia water is added to make the reaction environment alkaline. Preferably, the concentration of ammonia water in the reaction system is 0.10-0.50 g / L, and more preferably, the concentration of ammonia water in the reaction system is 0.25-0.35 g / L.
[0052] In some of the schemes, in step S1, the solvent is at least one of ethanol and water, preferably, the solvent is a mixed solvent of ethanol and water, further, the solvent is an ethanol-water mixed solvent with a volume ratio of 10:1-5, and more preferably, the solvent is an ethanol-water mixed solvent with a volume ratio of 10:3.
[0053] In some of the schemes, in step S1, the silicon source precursor is tetraethyl orthosilicate. Preferably, the silicon source precursor is mixed with ethanol to obtain a silicon source precursor reagent, and the silicon source precursor reagent is a tetraethyl orthosilicate-ethanol mixed solution with a volume ratio of 0.30-0.60mL:10mL. More preferably, the silicon source precursor reagent is a tetraethyl orthosilicate-ethanol mixed solution with a volume ratio of 0.45mL:10mL.
[0054] In some of the schemes, in step S1, the silicon source precursor is added by dropwise addition, preferably, the dropwise addition speed is 0.1-1 mL / min, more preferably, the dropwise addition speed is 0.5 mL / min.
[0055] In some of the schemes, in step S1, the usage ratio of the Fe3O4 nanomagnetic core to the silicon source precursor reagent is 0.3g:0.3-0.6mL, preferably 0.3g:0.4-0.5mL, and more preferably 0.3g:0.45mL.
[0056] In some of the schemes, in step S1, the reaction is carried out under an ultrasonic environment, preferably, the ultrasonic power is 30-50 KHz, preferably 45 KHz.
[0057] In some of the schemes, in step S3, the solvent is a PBS solution.
[0058] In some of the schemes, in step S3, the solvent of the Fe3O4@SiO2@polymer brush magnetic nanoparticle dispersion is water.
[0059] In some of the schemes, in step S3, the reaction is carried out at 10-40°C, preferably 20-30°C, more preferably 25°C.
[0060] In some of the schemes, in step S3, the reaction time is 10-30 h, preferably 15-20 h, and more preferably 17 h.
[0061] On the other hand, the present invention also discloses the application of the above-mentioned protease bioreactor in hydrolyzing peptide bonds.
[0062] In some of these schemes, the application includes use for enzymatic digestion of proteins, and / or, for detection of proteins;
[0063] When the protease bioreactor is used for enzymatic hydrolysis of protein, the protease bioreactor is added in an amount according to a mass ratio of protein to protease bioreactor of 1:50-200; preferably, the protein is first treated with urea and dithiothreitol, then treated with indoleacetic acid, and then added to the protease bioreactor for enzymatic hydrolysis;
[0064] When the protease bioreactor is used to detect protein, the steps include: adding the protease bioreactor in an amount according to a mass ratio of protein to protease bioreactor of 1:50-200, performing enzymatic hydrolysis, and performing mass spectrometry detection on the product obtained after enzymatic hydrolysis.
[0065] The above-mentioned “magnetic material” refers to a material that has the property of being attracted by an external magnetic field, such as ferrite material.
[0066] The above-mentioned "biocompatible materials" refer to materials that have a better affinity with proteins and will not cause protein denaturation or affect their functions, such as SiO2, Au, etc.
[0067] The above-mentioned "protease" refers to a protease responsible for hydrolyzing peptide bonds in proteins, such as trypsin and the like.
[0068] The above-mentioned "immobilized initiator" refers to a reagent that can be used to initiate a curing reaction, such as azobisisobutyronitrile, azocarbonyldiisobutyronitrile (Vazo 64), azopropionylhydrazide (ADH), azobutyronitrile (AIDN), and the like.
[0069] The above-mentioned "non-protonic polar solvent" refers to a solvent that has no protons in its molecules, is almost non-acidic compared to water, and has no amphoteric characteristics, but has a weaker tendency to accept protons and varying degrees of hydrogen bonding ability, such as N,N'-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, methyl-2-pyrrolidone, etc.
[0070] The above-mentioned "iron precursor" refers to a reagent that can obtain iron oxide, and can be selected according to the general requirements for preparing iron oxide in the art, such as ferrous chloride, ferric acetylacetonate, ferric chloride and iron oxide.
[0071] The above-mentioned “alkaline reagent” refers to a reagent that can make the reaction system alkaline, such as sodium acetate or sodium hydroxide.
[0072] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0073] The reagents and raw materials used in the present invention are commercially available.
[0074] The positive and progressive effects of the present invention are:
[0075] The protease bioreactor of the present invention uses a polymer brush to modify magnetic nanoparticles, which provides many active sites for protease immobilization and can improve the protease immobilization rate. The nitrogen lactone functional group in the polymer brush can react with the amino group or thiol group of trypsin, thereby enhancing its immobilization rate.
[0076] At the same time, since the polymer brush has a branched structure, the polymer-modified magnetic nanoparticles have a larger specific surface area, which increases the contact area between the protease and the substrate while improving the enzyme fixation rate, and the protease activity is also improved. Compared with the traditional immobilized enzyme using glutaraldehyde cross-linking agent, the immobilized protease in the present invention can eliminate the effect of glutaraldehyde toxicity on the protease activity, further improve the enzyme activity of the protease, and improve the coverage of the peptide segment after enzyme cleavage. The protease bioreactor provides an efficient, sustainable and environmentally friendly solution for enzyme catalysis reactions.
[0077] The method for using the protease bioreactor obtained by immobilizing protease with nano-magnetic particles is simpler. After the enzymatic hydrolysis of the protein is completed, the enzymatic hydrolysis product can be easily separated from the magnetic protease bioreactor by using a one-step magnetic separation. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is the electron microscope image of Fe3O4@SiO2@pVDMA;
[0079] Figure 2 The standard curve of trypsin. DETAILED DESCRIPTION
[0080] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0081] Abbreviations:
[0082] Urea (urea); DTT (dithiothreitol); IAA (indole-3-acetic acid); APTES (3-aminopropyltriethoxysilane).
[0083] Example 1
[0084] A protease bioreactor (i.e., Fe3O4@SiO2@pVDMA-trypsin) was prepared by the following method.
[0085] (1) Preparation of Fe3O4 nanomagnetic cores:
[0086] First, use an analytical balance to accurately weigh 0.5g of anhydrous FeCl3 powder into a 50mL conical flask. Add 20mL of ethylene glycol to the conical flask, and stir it with a magnetic stirrer at 1000rpm for 1 hour. After it is completely dissolved, weigh 0.2g of sodium citrate powder and add it to the conical flask, stir it with a magnetic stirrer at 1000rpm to make it completely dissolved, then add 0.2g of sodium acetate to it, and after it is completely dissolved, pour it into the lining of a polytetrafluoroethylene reactor, heat it at 200℃ for 10 hours, and magnetically separate it after the reactor is completely cooled to room temperature. The prepared Fe3O4 nano magnetic core is washed with ultrapure water several times until it is neutral, and a solution of Fe3O4 nano magnetic core is obtained, which is a Fe3O4 magnetic nanoparticle dispersion, and is stored at 4℃.
[0087] (2) Preparation of Fe3O4@SiO2 magnetic nanoparticles:
[0088] Take a Fe3O4 magnetic nanoparticle dispersion (containing 0.3 g Fe3O4 magnetic nanoparticles) and place it in a 250 mL round-bottom flask, discard the supernatant, add 100 mL of ethanol, 30 mL of purified water, and 0.15 mL of 25-28% (w / w) ammonia water to the flask, at which time the concentration of ammonia water in the reaction system is 0.26-0.31 g / L; install a mechanical stirring device on the ultrasonic instrument, set the ultrasonic time to 1 h, install the above-mentioned round-bottom flask, and ultrasonically treat the reaction system while stirring at a stirring speed of 200 rpm.
[0089] Take 0.45 mL of ethyl orthosilicate and dilute it with 10 mL of anhydrous ethanol, then add it to the constant pressure dropping funnel. After the device is ultrasonically reacted for 1 hour, install a constant pressure dropping funnel on the flask, add the ethyl orthosilicate / ethanol mixture dropwise (dropping speed is about 0.5 mL / min) to the reaction system, and continue to react with stirring and ultrasonication (ultrasonic power is 45KHz). After the reaction is completed, dismantle the reaction device, first collect the magnetic beads with a magnetic separator, wash them with ultrapure water several times until neutral, and finally obtain the Fe3O4@SiO2 magnetic nanoparticle dispersion, which is stored at 4°C.
[0090] (3) Preparation of Fe3O4@SiO2@pVDMA magnetic nanoparticles:
[0091] Fe3O4@SiO2 magnetic nanoparticle dispersion (containing 0.12 g Fe3O4@SiO2 magnetic nanoparticles) was placed in a 100 mL round-bottom flask, the supernatant was discarded and 30 mL ethanol was added, 120 μL 3-mercaptopropyltrimethoxysilane (1.2 mmol / L) was added to the round-bottom flask, and stirred for 12 h at room temperature (20-30 ° C). After washing with ultrapure water several times until neutral, the magnetic nanoparticles were transferred to a 500 mL round-bottom flask, the supernatant was discarded by magnetic attraction, 200 mL N,N'-dimethylformamide solvent was added, and then 800 mg azobisisobutyronitrile was added. Finally, 100 mL of 1 mmol / L 2-vinyl-4,4-dimethyl-2-oxazolin-5-one (VDMA, CAS: 29513-26-6, purchased from Shanghai Titan Technology Co., Ltd.), a mechanical stirring device was installed on the oil bath, the oil bath temperature was set to 70°C, the above round-bottom flask was installed, and the reaction system was heated while stirring at a stirring speed of 200 rpm, and heated and stirred for 17 h. After the reaction was completed, the reaction device was dismantled, the magnetic beads were first collected with a magnetic separator, and then washed with ultrapure water several times until neutral, and finally the Fe3O4@SiO2@pVDMA magnetic nanoparticle dispersion was obtained and stored at 4°C. The electron microscope image of the Fe3O4@SiO2@pVDMA is shown in the figure Figure 1 shown.
[0092] (4) Fe3O4@SiO2@pVDMA immobilized trypsin
[0093] Trypsin (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., CAS: 9002-07-7) was completely dissolved in 50 mM PBS, and 1 mL of 2 mg / mL trypsin solution was added to 1 mL of 10 mg / mL Fe3O4@SiO2@pVDMA magnetic nanoparticle solution, that is, the mass ratio of Fe3O4@SiO2@pVDMA to protease was 1:0.2, and oscillated at 25°C for 17 h using a 1000 rpm vortex oscillator. After the oscillation, the magnetic nanoparticles of the immobilized enzyme were separated by magnetic separation, and washed three times with ultrapure water to achieve the immobilization of trypsin, obtaining Fe3O4@SiO2@pVDMA-trypsin, which was stored at 4°C and counted as Fe3O4@SiO2@pVDMA-trypsin-1.
[0094] Example 2
[0095] A protease bioreactor (Fe3O4@SiO2@pGMA-trypsin) was prepared by the following method:
[0096] (1) Preparation of Fe3O4 magnetic nanoparticles: prepared according to the method of Example 1.
[0097] (2) Preparation of Fe3O4@SiO2 magnetic nanoparticles: prepared according to the method of Example 1.
[0098] (3) Preparation of Fe3O4@SiO2@pGMA magnetic nanoparticles:
[0099] The Fe3O4@SiO2 magnetic nanoparticle dispersion (containing 0.12 g Fe3O4@SiO2 magnetic nanoparticles) was placed in a 100 mL round-bottom flask, the supernatant was discarded and 30 mL ethanol was added. 120 μL 3-mercaptopropyltrimethoxysilane (1.2 mmol / L) was added to the round-bottom flask, and stirred at room temperature (20-30°C) for 12 h. After washing with ultrapure water several times until neutral, the magnetic nanoparticles were transferred to a 500 mL round-bottom flask, the supernatant was discarded by magnetic attraction, 200 mL N,N'-dimethylformamide solvent was added, and 800 mg azobisisobutyronitrile, and finally add 100μL of 1mmol / L glycidyl methacrylate (GMA, CAS: 106-91-2, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.), install a mechanical stirring device on the oil bath, set the oil bath temperature to 70℃, install the above round-bottom flask, and heat the reaction system while stirring at a stirring speed of 200rpm, and heat and stir for 17 hours. After the reaction is completed, dismantle the reaction device, first collect the magnetic beads with a magnetic separator, wash them with ultrapure water several times until neutral, and finally obtain the Fe3O4@SiO2@pGMA magnetic nanoparticle dispersion, which is stored at 4℃.
[0100] (4) Immobilization of trypsin by Fe3O4@SiO2@pGMA: Immobilization of trypsin was achieved by referring to the method of Example 1 to obtain Fe3O4@SiO2@pGMA-trypsin, which was then stored at 4°C.
[0101] Example 3
[0102] A protease bioreactor, denoted as Fe3O4@SiO2@pVDMA-trypsin-3, was prepared according to the method of Example 1, and the only difference from Example 1 was that in step (4), 0.5 mL of 2 mg / mL trypsin solution was added to 1 mL of 10 mg / mL Fe3O4@SiO2@pVDMA magnetic nanoparticle solution, that is, the mass ratio of nanomagnetic core@biocompatible layer@polymer brush to protease was 1:0.1.
[0103] Example 4
[0104] A protease bioreactor, denoted as Fe3O4@SiO2@pVDMA-trypsin-4, was prepared according to the method of Example 1, and the only difference from Example 1 was that in step (4), 5 mL of 2 mg / mL trypsin solution was added to 1 mL of 10 mg / mL Fe3O4@SiO2@pVDMA magnetic nanoparticle solution, that is, the mass ratio of nanomagnetic core@biocompatible layer@polymer brush to protease was 1:1.
[0105] Example 5
[0106] A method for enzymatic hydrolysis of plasma proteins, comprising the following steps:
[0107] Take 10 μL of the plasma sample diluted 100 times, add 50 μL of 8M urea, 20mM DTT in 1×PBS, incubate at 37°C at 1700 rpm for 1 h, add 20 μL of 0.2M IAA in 1×PBS, incubate at 25°C at 1700 rpm in the dark for 0.5 h, add 130 μL of Fe3O4@SiO2@pVDMA-trypsin of Example 1, 3 or 4 or Fe3O4@SiO2@pGMA-trypsin of Example 2, so that the mass ratio of protein / protease bioreactor (Fe3O4@SiO2@pVDMA-trypsin or Fe3O4@SiO2@pGMA-trypsin) is 1:50-200, dissolve in 25 mM ammonium bicarbonate solution, incubate at 37°C at 1700 rpm for 17 h. Magnetic Fe3O4@SiO2@pVDMA-trypsin or Fe3O4@SiO2@pGMA-trypsin is attracted and the supernatant solution is absorbed to complete the enzymatic hydrolysis of plasma proteins.
[0108] Example 6
[0109] A method for detecting plasma protein, using the Fe3O4@SiO2@pVDMA-trypsin of Example 1, 3 or 4 or the Fe3O4@SiO2@pGMA-trypsin of Example 2, comprises the following steps:
[0110] (1) Enzymatic hydrolysis: According to the method of Example 3, enzymatic hydrolysis of plasma protein is completed.
[0111] (2) Desalting and acidification: Take a desalting pipette tip (Thermo, 87784), aspirate 100 μL 50% acetonitrile (ACN) for activation, discard the waste liquid and aspirate 100 μL 5% trifluoroacetic acid (TFA) for acidification; slowly adsorb 200 μL of the enzymatic hydrolysate of step (1) onto the desalting pipette tip, aspirate 100 μL 0.1% trifluoroacetic acid (TFA) to desalt, elute with 50 μL 20% acetonitrile (ACN), 0.1% FA, elute with 50 μL 80% acetonitrile (ACN), 0.1% FA five times, elute with 50 μL 80% acetonitrile (ACN), 0.1% formic acid (FA), collect the supernatant and set aside;
[0112] (3) Mass spectrometry analysis: Take the supernatant obtained in step (2) and perform detection on a mass spectrometer in the conventional manner.
[0113] Comparative Example 1
[0114] A protease bioreactor (Fe3O4@SiO2-CHO-trypsin) was prepared by the following method:
[0115] (1) Preparation of Fe3O4@SiO2 magnetic nanoparticles: prepared according to the method of Example 1.
[0116] (2) Preparation of amination-modified Fe3O4@SiO2 magnetic nanoparticles:
[0117] Add 90 μL of 3-aminopropyltriethoxysilane (APTES) to 30 mL of a dispersion containing 200 mg of Fe3O4@SiO2 magnetic nanoparticles and shake at room temperature for 12 h; wash the product alternately with ultrapure water and ethanol for 5 times to obtain Fe3O4@SiO2-NH2 nanoparticles.
[0118] (3) Immobilization of trypsin by amination of Fe3O4@SiO2:
[0119] To 0.02 g of Fe3O4@SiO2-NH2, glutaraldehyde (2% v / v) dissolved in 33.33 mL of phosphate buffer (50 mM, pH 7.6) was added, and the mixture was shaken at 200 rpm for 2 h at room temperature, and then washed thoroughly with phosphate buffer; 1 mL of trypsin (1-2 mg / mL, pH 7.5 in phosphate buffer) was added to the above-mentioned Fe3O4@SiO2-NH2 magnetic nanoparticles treated with glutaraldehyde; after shaking at 200 rpm for 4 hours at room temperature, it was placed in a 4°C refrigerator for solidification for 16 hours; the product was magnetically separated and washed with phosphate buffer (pH 7.5) to obtain Fe3O4@SiO2-CHO-trypsin.
[0120] Experimental Example 1
[0121] The protease immobilization rate of the nanoparticles prepared in the above examples and comparative examples was tested.
[0122] The BCA kit (Thermo Fisher Scientific Inc. Micro BCA Protein Assay Kit) and trypsin were used to reduce divalent copper ions to monovalent copper ions under alkaline conditions, and the monovalent copper ions formed a purple complex with the BCA molecule. The purple complex has ultraviolet absorption at a wavelength of 540-590 nm, so the fixation rate of trypsin was calculated based on the color development principle of the BCA kit.
[0123] Establishment of standard curve: Take free trypsin, use PBS buffer (10×) to prepare trypsin solution (0, 30, 60, 90, 120, 150, 180 μg / mL), use BCA kit to develop color, use microplate reader to measure the absorbance of different trypsin solutions at 562 nm wavelength, and draw standard curve, such as Figure 2 As shown, the regression equation is calculated and the regression equation formula is as follows:
[0124] Y = 0.003X + 0.0744 (R 2 = 0.994)
[0125] Experimental plan: Take 1 mL of Fe3O4@SiO2@pVDMA-trypsin-1, Fe3O4@SiO2@pVDMA-trypsin-3, Fe3O4@SiO2@pVDMA-trypsin-4, Fe3O4@SiO2@ pGMA-trypsin and Fe3O4@SiO2-CHO-trypsin respectively and place them in 2 mL centrifuge tubes. Use a magnetic stand for magnetic absorption, take the supernatant, and use the BCA kit to determine the content of trypsin in the supernatant at a wavelength of 562 nm. According to the amount of trypsin input minus the content of trypsin in the supernatant, the fixation rate of trypsin is obtained, and the calculation formula is as follows:
[0126] Fixation rate (%) = ( A - B ) / A × 100 %
[0127] Where A is the initial concentration of trypsin (mg / mL); B is the concentration of trypsin in the supernatant (mg / mL).
[0128] The enzyme fixation rate of the protease bioreactor prepared in the above examples and comparative examples was analyzed, and the results are as follows:
[0129] Table 1. Enzyme immobilization rate
[0130]
[0131] The above results show that compared with the traditional use of glutaraldehyde crosslinker to immobilize trypsin, the use of polymer brush-modified Fe3O4@SiO2 magnetic nanoparticles to immobilize trypsin has a higher enzyme fixation rate, especially when the polymer brush is pVDMA, the fixation rate of trypsin reaches 100%. This shows that polymer brush-modified Fe3O4@SiO2 magnetic nanoparticles can provide more binding sites for trypsin and improve the enzyme fixation rate.
[0132] Moreover, when the amount of trypsin is increased or decreased, the fixation rate of trypsin will decrease. Too high an amount of trypsin may lead to increased interactions between enzyme molecules, making the enzyme unevenly fixed on the surface of the magnetic beads, thereby reducing the fixation rate. Too low an amount of trypsin may not be able to fully cover the surface of the magnetic beads, resulting in failure to effectively fix to the magnetic beads, thereby reducing the fixation rate.
[0133] Experimental Example 2
[0134] The protease enzymatic activity of the nanoparticles prepared in the above examples and comparative examples was tested.
[0135] Trypsin catalyzes the hydrolysis of the ester bond of N-benzoyl-L-arginine ethyl ester (BAEE) to generate N-benzoyl-L-arginine (BA). BA has a characteristic absorption peak at 253 nm. The activity of trypsin can be calculated by measuring the rate of increase of absorbance at 253 nm.
[0136] Experimental plan: 1 mL of free trypsin, Fe3O4@SiO2@pVDMA-trypsin-1, Fe3O4@SiO2@pVDMA-trypsin-3, Fe3O4@SiO2@pVDMA-trypsin-4, Fe3O4@SiO2-CHO-trypsin and Fe3O4@SiO2@pGMA-trypsin were placed in 2 mL centrifuge tubes, and the trypsin activity was determined using a trypsin activity detection kit (Beijing Solebow Technology Co., Ltd.). The change in absorbance of the test object at a wavelength of 253 nm within 1 min was measured, and the enzyme activity was calculated using the following formula:
[0137] Trypsin activity (U / mg) = ΔA × V / (0.001 × V × C × T)
[0138] Where ΔA is the change in enzyme absorbance during the reaction time; Vreaction is the total volume of the reaction (mL); Vsample is the added sample volume (mL); C is the enzyme concentration (mg / mL); and T is the reaction time (s).
[0139] The enzyme activity analysis of the protease bioreactors prepared in the above Examples 1-4 and Comparative Example 1 was performed, and the results are as follows:
[0140] Table 2. Enzymatic activity
[0141]
[0142] The results showed that compared with free trypsin, the activity of Fe3O4@SiO2-CHO-trypsin was slightly decreased, while the activity of Fe3O4@SiO2@pVDMA-trypsin-1, Fe3O4@SiO2@pVDMA-trypsin-3, Fe3O4@SiO2@pVDMA-trypsin-4 and Fe3O4@SiO2@pGMA-trypsin modified with polymer brushes was improved, indicating that the polymer brush-VDMA-modified Fe3O4@SiO2 magnetic nanoparticles provide more binding sites for trypsin, while increasing the contact area between trypsin and substrate, thereby increasing the activity of trypsin.
[0143] Moreover, when the dosage of trypsin was increased or decreased, the enzyme activity of Fe3O4@SiO2@pVDMA-trypsin decreased. This may be because when the enzyme dosage was too high, the interaction between enzyme molecules increased during the fixation process, the enzyme molecular structure changed or inactivated, and then the activity of the enzyme on the magnetic beads was reduced; when the enzyme dosage was too low, the enzyme density on the surface of the magnetic beads was insufficient, and the failure to achieve sufficient enzyme coverage limited the contact between the enzyme and the substrate, thereby reducing its activity.
[0144] In particular, the Fe3O4@SiO2 magnetic nanoparticle-immobilized trypsin reactor (Fe3O4@SiO2@pVDMA-trypsin-1) modified with VDMA polymer brushes exhibited the highest enzyme activity, which was 3.95 times that of free trypsin, 6 times that of Fe3O4@SiO2-CHO-trypsin, and 3.38 times that of Fe3O4@SiO2@pGMA-trypsin.
[0145] Experimental Example 3
[0146] The peptide coverage of the protease bioreactor prepared in the above examples and comparative examples was tested.
[0147] 1 μL of free trypsin, Fe3O4@SiO2@pVDMA-trypsin-1, Fe3O4@SiO2@pVDMA-trypsin-3, Fe3O4@SiO2@pVDMA-trypsin-4, Fe3O4@SiO2-CHO-trypsin and Fe3O4@SiO2@pGMA-trypsin were taken and mixed with plasma. The peptide concentration was measured at A205 on Nano Drop ND300 and mass spectrometry was performed according to the method of Example 3. The peptide coverage was calculated using DIA-NN open source software (Cambridge Centre for Proteomics) according to its instructions.
[0148] The protease bioreactors prepared in the above examples and comparative example 1 were subjected to peptide coverage analysis, and the results are as follows:
[0149] Table 3. Peptide coverage results
[0150]
[0151] The results showed that compared with free trypsin, the peptide coverage of Fe3O4@SiO2-CHO-trypsin was lower, while the peptide coverage of Fe3O4@SiO2@pVDMA-trypsin-1, Fe3O4@SiO2@pVDMA-trypsin-3, Fe3O4@SiO2@pVDMA-trypsin-4 and Fe3O4@SiO2@pGMA-trypsin modified with polymer brushes was higher than that of free trypsin, indicating that the immobilization of trypsin on Fe3O4@SiO2 magnetic nanoparticles modified with polymer brushes enabled the enzyme to catalyze specific sites more selectively. A higher peptide coverage usually means that more peptides were successfully detected and identified, which means that the enzymatic cleavage produced more peptides, further illustrating the efficiency of the enzymatic cleavage.
[0152] Moreover, when the amount of trypsin was increased or decreased, the peptide coverage rate decreased. This may be because when the enzyme dosage was too high or too low, the activity of the enzyme on the magnetic beads decreased, resulting in some proteins not being fully digested, making some peptides unable to be detected, thereby reducing the peptide coverage rate.
[0153] In particular, after enzymatic hydrolysis of proteins using Fe3O4@SiO2 magnetic nanoparticles immobilized trypsin reactor (Fe3O4@SiO2@pVDMA-trypsin-1) modified with pVDMA polymer brushes, 13,626 proteins were detected with a peptide coverage of 74.5%.
Claims
1. A protease bioreactor, characterized in that The invention comprises a nanomagnetic core made of a magnetic material, a biocompatible layer made of a biocompatible material, a polymer brush and a protease, wherein the polymer brush is poly (2-vinyl-4,4-dimethyl-2-oxazoline-5-one); the biocompatible layer is coated on the outside of the nanomagnetic core, the polymer brush is grafted and modified on the biocompatible layer, the protease is covalently linked to the polymer brush to form nanoparticles of nanomagnetic core@biocompatible layer@polymer brush-protease, i.e. a protease bioreactor; the magnetic material is Fe3O4, the biocompatible material is SiO2, the protease is trypsin, and the mass ratio of the nanomagnetic core@biocompatible layer@polymer brush to the protease is 1:0.18-0.
22.
2. The protease bioreactor according to claim 1, characterized in that The particle size of the nano magnetic core is 10nm-1μm; And / or, the thickness of the biocompatible layer is 5-10 nm; And / or, the polymer brush has a thickness of 10-50 nm.
3. The method for preparing a protease bioreactor according to any one of claims 1 to 2, characterized in that: The nanoparticles are Fe3O4@SiO2@polymer brush-protease, comprising the following steps: Preparation of S1, Fe3O4@SiO2 magnetic nanoparticles: Fe3O4 nano-magnetic cores are dispersed in a solvent, and a silicon source precursor is added in an alkaline environment to react and obtain Fe3O4@SiO2 magnetic nanoparticles; Preparation of S2, Fe3O4@SiO2@polymer brush magnetic nanoparticles: Fe3O4@SiO2 magnetic nanoparticles are dispersed in a solvent, a thiolating agent is added to carry out a thiolating reaction, the system solvent is replaced with a non-protonic polar solvent, and then an immobilized initiator and a polymer brush monomer are added to carry out an atom transfer radical polymerization reaction to obtain Fe3O4@SiO2@polymer brush magnetic nanoparticles; Preparation of S3, Fe3O4@SiO2@polymer brush-protease nanoparticles: The protease is dissolved in a solvent to obtain a protease solution, and the protease solution is added into a Fe3O4@SiO2@polymer brush magnetic nanoparticle dispersion to allow the protease to react with the Fe3O4@SiO2@polymer brush magnetic nanoparticles and be fixed on the Fe3O4@SiO2@polymer brush magnetic nanoparticles.
4. The method for preparing a protease bioreactor according to claim 3, characterized in that: In step S2, the immobilized initiator is azobisisobutyronitrile; And / or, in step S2, the aprotic polar solvent is N,N'-dimethylformamide; and / or, in step S2, the polymer brush monomer is 2-vinyl-4,4-dimethyl-2-oxazoline-5-one; and / or, in step S2, the dosage ratio of the Fe3O4@SiO2 magnetic nanoparticles to the polymer brush monomer is 12 g: 1-100 mmol; And / or, in step S2, the mass ratio of the Fe3O4@SiO2 magnetic nanoparticles to the immobilized initiator is 120:600-1000; and / or, in step S2, the atom transfer radical polymerization reaction is carried out at 50-90° C.; And / or, in step S2, the atom transfer radical polymerization reaction time is 10-30h; And / or, in step S2, the solvent is ethanol; And / or, in step S2, the thiol-forming agent is 3-mercaptopropyltrimethoxysilane; and / or, in step S2, the thiolation reaction is carried out at 10-40° C.; And / or, in step S2, the thiolation reaction time is 8-16 hours.
5. The method for preparing a protease bioreactor according to claim 3, characterized in that: Before step S1, the following step S0 is also included: Preparation of S0, Fe3O4 nano magnetic cores: Mix a mixed solution containing an iron precursor and a reducing agent with an alkaline reagent in a solvent, heat and react to obtain the obtained product.
6. The method for preparing a protease bioreactor according to claim 5, characterized in that: In step S0, the temperature of the heating reaction is 190-220°C; And / or, in step S0, the heating reaction time is 6-72h; And / or, in step S0, the iron precursor is ferric chloride; And / or, in step S0, the reducing agent is sodium citrate; And / or, in step S0, the molar ratio of the iron precursor to the reducing agent is 2-6:1; And / or, in step S0, the alkaline reagent is sodium acetate; And / or, in step S0, the molar ratio of the iron precursor to the alkaline reagent is 1.0-2.0:1; And / or, in step S0, the solvent is ethylene glycol; And / or, in step S1, before adding the silicon source precursor, adding ammonia water to treat the reaction environment to make it alkaline, and the concentration of the ammonia water in the reaction system is 0.10-0.50 g / L; And / or, in step S1, the solvent is a mixed solvent of ethanol and water, and the solvent is an ethanol-water mixed solvent with a volume ratio of 10:1-5; And / or, in step S1, the silicon source precursor is tetraethyl orthosilicate; And / or, in step S1, the silicon source precursor is mixed with ethanol to obtain a silicon source precursor reagent, and the silicon source precursor reagent is a ethyl orthosilicate-ethanol mixed solution with a volume ratio of 0.30-0.60 mL:10 mL; And / or, in step S1, the silicon source precursor is added dropwise, and the dropping speed is 0.1-1 mL / min; And / or, in step S1, the usage ratio of the Fe3O4 nano-magnetic core to the silicon source precursor is 0.3g:0.3-0.6mL; And / or, in step S1, the reaction is carried out under an ultrasonic environment; And / or, in step S3, the solvent is a PBS solution; and / or, in step S3, the solvent of the Fe3O4@SiO2@polymer brush magnetic nanoparticle dispersion is water; And / or, in step S3, the reaction is carried out at 10-40°C; And / or, in step S3, the reaction time is 10-30h.
7. Use of the protease bioreactor according to any one of claims 1 to 2 in hydrolyzing peptide bonds.
8. The use according to claim 7, characterized in that The application includes enzymatic digestion of proteins, and / or detection of proteins; When the protease bioreactor is used for enzymatic hydrolysis of proteins, the protease bioreactor is added in an amount according to a mass ratio of protein to protease bioreactor of 1:50-200 to perform enzymatic hydrolysis; When the protease bioreactor is used to detect protein, the steps include: adding the protease bioreactor in an amount according to a mass ratio of protein to protease bioreactor of 1:50-200, performing enzymatic hydrolysis, and performing mass spectrometry detection on the product obtained after enzymatic hydrolysis.