A kind of preparation method of malononitrile

By using modified cobalt cerium copper aluminum hydrotalcite catalyst in the preparation of malononitrile, the problems of low yield and insufficient catalyst activity in the existing process are solved, and efficient and economical preparation of malononitrile is achieved, which is suitable for industrial applications.

CN118619847BActive Publication Date: 2024-10-22YUANCATALYST TECHNOLOGY (SHENYANG) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411099885.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-10-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing malononitrile preparation process has problems such as low yield, complex process and low catalyst activity, making it difficult to meet the needs of industrial production.

Method used

By ultrasonic dispersion of metal salts such as cobalt, cerium, copper and aluminum and then hydrothermal reaction, a mixture of hydrotalcite-like, TS-1 and gibbsite is prepared, spray granulation is performed to prepare a catalyst with excellent catalytic activity, and the catalyst is added to the catalyst bed It reacts with ammonia gas in the layer to achieve efficient preparation of malononitrile.

Benefits of technology

The activity and life of the catalyst are significantly improved, the yield of malononitrile reaches more than 98%, the process is simple, suitable for industrial production, and the cost of treating three wastes is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of fine chemicals, and in particular to a method for preparing malononitrile. The preparation method comprises the following steps: a raw material is introduced into a catalyst bed together with ammonia gas for reaction. Wherein, a hydrotalcite-like substance containing cobalt, cerium, copper and aluminum is prepared, and TS-1, gibbsite and an appropriate amount of water are ground and mixed to obtain a slurry, and then spray granulated and roasted to obtain a catalyst. The catalyst obtained by spray granulation of a hydrotalcite-like substance with TS-1, gibbsite and the like in the present invention has excellent catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of fine chemicals and more specifically relates to a method for preparing malononitrile. Background Art

[0002] Malononitrile is a fine chemical product and a synthetic raw material for pharmaceutical vitamin B1 and pesticides. In recent years, the application of organic conductive materials based on tetracyano compounds made from malononitrile in the electrical field has also received increasing attention. The industrial preparation of malononitrile generally uses cyanoacetic acid as a raw material, which has a complex process, high cost, and a lot of waste, and can no longer meet the needs of current industrial production.

[0003] CN116143657A discloses a method for synthesizing malononitrile by using acetonitrile and cyanogen chloride as raw materials, reacting in a fixed bed reactor containing a solid base catalyst, separating a crude product and unreacted raw materials by condensation, recycling the unreacted raw materials, and distilling the crude product to obtain malononitrile. The present invention has the advantages of mild reaction conditions, simple process, convenient operation, low cost, less three wastes, and easy industrial production. However, the yield of the preparation process is not high, and the process is complicated.

[0004] CN112724041A discloses a method for preparing malononitrile and the malononitrile prepared, wherein the preparation method comprises the following steps: mixing cyanoacetamide, a catalyst and a solvent, heating to reflux and introducing phosgene to synthesize malononitrile; wherein the mass ratio of cyanoacetamide, the catalyst and the solvent is (2.5-3.5): (0.005-0.02): (7.5-10.5); the solvent is any one of dichloromethane, dichloroethane or toluene; the catalyst is any one or more of diethylamine, N, N-dimethylformamide or pyridine. The present invention uses cyanoacetamide to synthesize malononitrile in the next step under the action of phosgene, the required raw materials are cheap and easy to obtain, and the synthetic reaction steps are few, there are no harsh conditions, the operation is simple, stable and controllable, the yield of the prepared malononitrile can reach more than 93%, which is much higher than other process schemes, and the preparation method of the present invention has low cost for three waste treatment and has objective economic benefits.

[0005] CN110590601A discloses a method for synthesizing malononitrile, the steps of which are as follows: adding dichloromethane and sodium cyanide to a reactor in a molar ratio of 1:1 to 3:1, slowly adding a catalyst to the reactor under stirring and heating conditions, controlling the temperature in the reactor at 90°C, and continuing to keep warm for 5-9 hours after the addition is completed; adding deionized water to the reaction product to wash the organic phase multiple times, separating the organic phase, drying the organic phase, and rectifying to obtain malononitrile; the catalyst is a combination of aluminum trichloride and tetrabutylammonium bromide. The present invention uses cheap dichloromethane as a raw material to directly synthesize malononitrile products in a one-step method, with a simple process route and low cost.

[0006] The preparation process in the prior art is complicated, or the yield of malononitrile is low, or the activity of the catalyst is not high. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the prior art and provide a method for preparing malononitrile. The preparation method comprises the following steps: the raw materials and ammonia are introduced into a catalyst bed for reaction. Among them, a hydrotalcite-like substance containing cobalt, cerium, copper and aluminum is prepared and ground and mixed with TS-1, gibbsite and an appropriate amount of water to obtain a slurry, and then spray granulated and roasted to obtain a catalyst. The catalyst obtained by spray granulation of a hydrotalcite-like substance with TS-1, gibbsite and the like in the present invention has excellent catalytic activity.

[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0009] A method for preparing malononitrile, the preparation method comprising the following steps:

[0010] The raw materials and ammonia gas are introduced into the catalyst bed for reaction.

[0011] Preferably, the raw material is malonic acid or dimethyl malonate.

[0012] Further preferably, the reaction conditions of the reaction are: the molar ratio of the raw material to the ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-2 h -1 ; The reaction temperature is 350~450℃.

[0013] In the present invention, a preferred solution is that the raw material is preheated before entering the catalyst bed together with ammonia, and the preheating temperature is 140-180°C.

[0014] In the present invention, in a further preferred embodiment, the method for preparing the catalyst comprises the following steps:

[0015] (1) Weighing cobalt salt, cerium salt, copper salt and aluminum salt, ultrasonically dispersing them in deionized water to prepare a mixed salt solution, then dropping alkali solution to adjust the pH of the solution, then transferring the solution to a hydrothermal reactor for reaction, centrifuging, washing, drying and grinding to obtain a hydrotalcite-like substance;

[0016] (2) The hydrotalcite-like substance, TS-1, gibbsite and an appropriate amount of water obtained in step (1) are ground and mixed to obtain a slurry, which is then spray-granulated and calcined at 550-650° C. for 4-8 hours to obtain a catalyst.

[0017] Preferably, in step (1), the pH is 9-11; the hydrothermal reaction is carried out at 130-150° C. for 6-12 h; and the drying is carried out at 80-120° C. for 8-16 h.

[0018] Preferably, in step (1), the cobalt salt is at least one of cobalt nitrate, cobalt chloride and cobalt acetate; the cerium salt is at least one of cerium acetate, cerium chloride and cerium nitrate; the copper salt is at least one of copper nitrate, copper acetate and copper chloride; the aluminum salt is at least one of aluminum acetate, aluminum chloride and aluminum nitrate.

[0019] Preferably, in step (1), the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.2-0.4.

[0020] Preferably, in step (1), in step (1), the molar ratio of the cobalt salt, the cerium salt, the copper salt and the aluminum salt is 2:0.1~0.2:0.05~0.15:1~2: the concentration of the alkali solution is 2~3 mol / L.

[0021] Preferably, in step (2), the mass ratio of the hydrotalcite-like substance, TS-1, and gibbsite is 0.4-0.6:0.5-0.9:1.

[0022] In the present invention, a preferred technical solution is a method for preparing malononitrile, which comprises the following steps:

[0023] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0024] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0025] S3, after the raw materials are metered, they enter the preheating section through the feeder, and after preheating, they enter the catalyst bed together with ammonia gas to react;

[0026] S4. The crude product is purified by distillation to obtain the product malononitrile.

[0027] The present invention has the following beneficial effects:

[0028] (1) The present invention modifies the cobalt-aluminum hydrotalcite by cerium and copper, and utilizes the interaction between the cerium and copper modified components to significantly improve the catalytic performance of the catalyst.

[0029] (2) By mixing hydrotalcite with TS-1 and gibbsite and spray granulating, the life of the catalyst is improved, as well as the catalyst activity and the yield of the final product.

[0030] (3) The raw materials of the catalyst of the present invention are widely available and the preparation process is simple, which is conducive to industrial production. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0033] Example 1

[0034] A method for preparing a catalyst comprises the following steps:

[0035] (1) Weigh 2 mol of cobalt nitrate, 0.15 mol of cerium chloride, 0.1 mol of copper nitrate and 1.5 mol of aluminum acetate and ultrasonically disperse them in 300 mL of deionized water to prepare a mixed salt solution, then dropwise add 2.5 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3) to adjust the pH of the solution to 10, then transfer to a hydrothermal reactor and react at 140°C for 10 h, centrifuge, wash, dry at 100°C for 12 h, and grind to obtain a hydrotalcite-like substance;

[0036] (2) 50 g of the hydrotalcite obtained in step (1), 70 g of TS-1, 100 g of gibbsite and an appropriate amount of water were ground and mixed to obtain a slurry, which was then spray-granulated and calcined at 600°C for 6 h to obtain a catalyst.

[0037] Example 2

[0038] A method for preparing a catalyst comprises the following steps:

[0039] (1) Weigh 2 mol of cobalt chloride, 0.2 mol of cerium nitrate, 0.05 mol of copper acetate and 2 mol of aluminum chloride, ultrasonically disperse them in 300 mL of deionized water to prepare a mixed salt solution, then dropwise add 2.5 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3) to adjust the pH of the solution to 11, then transfer to a hydrothermal reactor and react at 150°C for 6 h, centrifuge, wash, dry at 120°C for 8 h, and grind to obtain hydrotalcite-like substance;

[0040] (2) 60 g of the hydrotalcite obtained in step (1), 50 g of TS-1, 100 g of gibbsite and an appropriate amount of water were ground and mixed to obtain a slurry, which was then spray granulated and calcined at 650°C for 4 h to obtain a catalyst.

[0041] Example 3

[0042] A method for preparing a catalyst comprises the following steps:

[0043] (1) Weigh 2 mol of cobalt acetate, 0.1 mol of cerium nitrate, 0.15 mol of copper chloride and 1 mol of aluminum nitrate, ultrasonically disperse them in 300 mL of deionized water to prepare a mixed salt solution, then dropwise add 2.5 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3) to adjust the pH of the solution, then transfer to a hydrothermal reactor and react at 130°C for 12 h, centrifuge, wash, dry at 80°C for 16 h, and grind to obtain hydrotalcite-like;

[0044] (2) 40 g of the hydrotalcite obtained in step (1), 90 g of TS-1, 100 g of gibbsite and an appropriate amount of water were ground and mixed to obtain a slurry, which was then spray-granulated and calcined at 550-650°C for 4-8 h to obtain a catalyst.

[0045] Comparative Example 1

[0046] A method for preparing a catalyst comprises the following steps:

[0047] (1) Weigh 2 mol of cobalt nitrate, 0.25 mol of cerium chloride and 1.5 mol of aluminum acetate and ultrasonically disperse them in 300 mL of deionized water to prepare a mixed salt solution, then dropwise add 2.5 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3) to adjust the pH of the solution to 10, then transfer to a hydrothermal reactor and react at 140°C for 10 hours, centrifuge, wash, dry at 100°C for 12 hours, and grind to obtain a hydrotalcite-like substance;

[0048] (2) 50 g of the hydrotalcite obtained in step (1), 70 g of TS-1, 100 g of gibbsite and an appropriate amount of water were ground and mixed to obtain a slurry, which was then spray-granulated and calcined at 600°C for 6 h to obtain a catalyst.

[0049] Comparative Example 2

[0050] A method for preparing a catalyst comprises the following steps:

[0051] (1) Weigh 2 mol of cobalt nitrate, 0.15 mol of cerium chloride, 0.1 mol of copper nitrate and 1.5 mol of aluminum acetate and ultrasonically disperse them in 300 mL of deionized water to prepare a mixed salt solution, then dropwise add 2.5 mol / L alkali solution (the alkali is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.3) to adjust the pH of the solution to 10, then transfer to a hydrothermal reactor and react at 140°C for 10 h, centrifuge, wash, dry at 100°C for 12 h, and grind to obtain a hydrotalcite-like substance;

[0052] (2) 50 g of the hydrotalcite obtained in step (1), 170 g of gibbsite and an appropriate amount of water were ground and mixed to obtain a slurry, which was then spray-granulated and calcined at 600° C. for 6 h to obtain a catalyst.

[0053] Comparative Example 3

[0054] A method for preparing a catalyst comprises the following steps:

[0055] ) Grind and mix 120g TS-1, 100g gibbsite and an appropriate amount of water to obtain a slurry, which is then spray-granulated and calcined at 600°C for 6h to obtain a catalyst.

[0056] The catalytic effects of Examples 1-3 and Comparative Examples 1-5 were tested, wherein the lifespan of the catalysts of Examples 1-3 and Comparative Examples 2-3 was tested. The specific test results are shown in Table 1.

[0057] A method for preparing malononitrile, the preparation method comprising the following steps:

[0058] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0059] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0060] S3, after being metered, malonic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 160°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:8; the reaction pressure is 2.2Mpa, and the raw material space velocity is 1.2h -1 ; Reaction temperature is 410℃

[0061] S4. The crude product is purified by distillation to obtain the product malononitrile.

[0062] Table 1:

[0063]

[0064] It can be seen from Table 1 that the active components supported by the present invention and the raw materials interact with each other. Under the presence of the joint action, the catalyst has a long life and excellent catalytic activity, and the yield of malononitrile is above 98%.

[0065] The yield of Test Example 1 under different reaction conditions is shown in Test Example 1-2.

[0066] Test Example 1: A method for preparing malononitrile, the preparation method comprising the following steps:

[0067] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0068] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0069] S3, after being metered, malonic acid enters the preheating section through the feeder, and after preheating, enters the catalyst bed together with ammonia to react; the preheating temperature is 180°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:19; the reaction pressure is 0.3Mpa, and the raw material space velocity is 1.9h -1 ; Reaction temperature is 445℃

[0070] S4, the crude product is purified by distillation to obtain the product malononitrile, wherein the yield of malononitrile is 99.2%.

[0071] Test Example 2:

[0072] A method for preparing malononitrile, the preparation method comprising the following steps:

[0073] S1, taking 1 kg of catalyst to prepare a catalyst bed;

[0074] S2, loading the catalyst bed prepared in step S1 into a fixed bed reactor;

[0075] S3, dimethyl malonate is metered and enters the preheating section through the feeder, and after preheating, it enters the catalyst bed together with ammonia to react; the preheating temperature is 140°C; the reaction conditions of the reaction are that the molar ratio of the raw material to the ammonia is 1:3; the reaction pressure is 4.9Mpa, and the raw material space velocity is 0.3h -1 ; Reaction temperature is 365℃

[0076] S4, the crude product is purified by distillation to obtain the product malononitrile, wherein the yield of malononitrile is 98.9%.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing malononitrile, characterized in that: The preparation method comprises the following steps: The raw materials and ammonia are introduced into the catalyst bed for reaction; The raw material is malonic acid or dimethyl malonate; The reaction conditions of the reaction are as follows: the molar ratio of the raw material to the ammonia is 1:2-20; the reaction pressure is 0.1-5 MPa, and the raw material space velocity is 0.1-2 h -1 ; Reaction temperature is 350~450℃; The preparation method of the catalyst comprises the following steps: (1) Weighing cobalt salt, cerium salt, copper salt and aluminum salt, ultrasonically dispersing them into deionized water to prepare a mixed salt solution, then dropping an alkali solution to adjust the pH of the solution, then transferring the solution to a hydrothermal reactor for reaction, centrifuging, washing, drying and grinding to obtain a hydrotalcite-like substance; the molar ratio of the cobalt salt, cerium salt, copper salt and aluminum salt is 2:0.1-0.2:0.05-0.15:1-2; (2) Grinding and mixing the hydrotalcite-like substance, TS-1, gibbsite and an appropriate amount of water obtained in step (1) to obtain a slurry, spray granulating the slurry, and calcining the slurry at 550-650° C. for 4-8 h to obtain a catalyst; the mass ratio of the hydrotalcite-like substance, TS-1, and gibbsite is 0.4-0.6:0.5-0.9:

1.

2. A method for preparing malononitrile according to claim 1, characterized in that: The raw material is preheated before entering the catalyst bed together with ammonia, and the preheating temperature is 140-180°C.

3. A method for preparing malononitrile according to claim 1, characterized in that: In step (1), the pH is 9-11; the hydrothermal reaction is carried out at 130-150° C. for 6-12 hours; and the drying is carried out at 80-120° C. for 8-16 hours.

4. A method for preparing malononitrile according to claim 1, characterized in that: In step (1), the cobalt salt is at least one of cobalt nitrate, cobalt chloride and cobalt acetate; the cerium salt is at least one of cerium acetate, cerium chloride and cerium nitrate; the copper salt is at least one of copper nitrate, copper acetate and copper chloride; the aluminum salt is at least one of aluminum acetate, aluminum chloride and aluminum nitrate.

5. A method for preparing malononitrile according to claim 1, characterized in that: In step (1), the alkali in the alkaline solution is sodium carbonate and sodium hydroxide; the molar ratio of sodium carbonate to sodium hydroxide is 1:0.2-0.

4.

6. A method for preparing malononitrile according to claim 1, characterized in that: In step (1), the concentration of the alkaline solution is 2-3 mol / L.

Citation Information

Patent Citations

  • Synthetic method of malononitrile

    CN110590601A

  • Preparation method of malononitrile and malononitrile prepared by preparation method

    CN112724041A

  • Synthesis method of malononitrile

    CN116143657A

  • Method for preparing adiponitrile through adipic acid gas phase ammonification and dehydration