Preparation method and application of composite heterostructure GDC@3D-MN Co3O4 material
Through the composite heterostructure GDC@3D-MN Co3O4 material, the problem of insufficient density of GDC materials is solved, and a high-density battery barrier layer is prepared at low sintering temperature, reducing ohmic impedance and improving ion conductivity, which is suitable for large Size battery and commercially prepared.
Patent Information
- Application Number
- CN202411154394.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Inadequate density of existing GDC materials leads to attenuation of battery performance, and high sintering temperature is required to improve density. However, this method is not suitable for large-size batteries and commercially prepared, and has a high ohmic impedance.
Using composite heterostructure GDC@3D-MN Co3O4 material, by combining Ce(NO3)3·6H2O and Gd(NO3)3·6H2O with 3D-MN Co3O4, NH4HCO3 is used as a precipitant to control the reduction of sintering temperature and improve the material density and ion conductivity.
It realizes the preparation of high-density battery barrier layers at lower sintering temperatures, reduces ohmic impedance and improves ion conductivity, and is suitable for large-size batteries and commercial preparation.
Smart Images

Figure CN118651899B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a composite heterostructure GDC@3D-MN Co3O4 material, belonging to the technical field of electrolytes containing cerium oxide. Background Art
[0002] In solid oxide batteries, a double-layer electrolyte structure of Y2O3-stabilized ZrO2 (YSZ) and Gd-doped CeO2 (GDC) is usually used. YSZ prevents electron leakage, and GDC prevents the common perovskite cathode from reacting with YSZ to form an insulating phase and affecting the performance of the battery. However, the pure GDC material has the defect of insufficient density, which will cause the battery performance to decay, reduce the ionic conductivity of the electrolyte, and increase the ohmic impedance of the battery. To achieve the ideal density, the sintering temperature required is too high.
[0003] Improving the compactness of the GDC barrier layer while reducing its sintering temperature is a technical problem that needs to be solved urgently in this field.
[0004] CN111574244A discloses a method for densifying a solid oxide battery barrier layer, wherein the GDC barrier layer is calcined at 1250°C for 3 hours, and then hydrothermally reacted with a nitric acid aqueous solution of the same components as GDC for 24 hours to obtain a dense GDC barrier layer. This method requires a hydrothermal reaction, is difficult to apply, is not suitable for large-size batteries and large-scale commercial preparation, and the ohmic impedance of the GDC barrier layer prepared by it is high. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a preparation method and application of a composite heterostructure GDC@3D-MN Co3O4 material to achieve the following invention objectives: the composite heterostructure GDC@3D-MN Co3O4 material has a low sintering temperature when preparing a battery barrier layer, and the prepared battery barrier layer has high density, high ion conductivity and low ohmic impedance.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A preparation method of a composite heterostructure GDC@3D-MN Co3O4 material comprises the following steps: dissolving Ce(NO3)3·6H2O and Gd(NO3)3·6H2O in deionized water to obtain a nitrate solution, adding 3D-MN Co3O4 to the nitrate solution, uniformly dispersing the solution, heating the solution to 57-63°C, slowly dropping an NH4HCO3 solution under stirring until the pH value of the solution is 7.5-8.0, standing the solution to obtain a white precipitate, and washing, drying, and calcining the solution to obtain a GDC@3D-MN Co3O4 powder material.
[0008] The molecular formula of the GDC is Ce 0.9 G 0.1 O 1.95 ;
[0009] The molar ratio of Ce(NO3)3·6H2O to Gd(NO3)3·6H2O is 8.8-9.2:1; the mass ratio of 3D-MN Co3O4 to Ce(NO3)3·6H2O is 1:1-4.
[0010] The concentration of the nitrate solution is 0.08-0.13 mol / L; the molar ratio of the 3D-MN Co3O4 to NH4HCO3 is 1:8.7-9.3.
[0011] The temperature was controlled at 57-63° C. during the dropwise addition of the NH 4 HCO 3 solution and the standing process.
[0012] The specific operation of washing and drying is: washing with deionized water and anhydrous ethanol for three times respectively by centrifugation, and then drying in an oven at 68-73° C. for 23.5-24.5 hours.
[0013] The calcination temperature is 745-755° C., and the calcination time is 1.7-2.3 hours.
[0014] The preparation method of the 3D-MN Co3O4 is as follows: N-CN is dispersed in a cobalt nitrate solution, and after being evenly dispersed, the obtained suspension is kept at 33-38°C for 11-13 hours; the suspension is then filtered, the filter cake is washed, and dried, and the obtained dry product is heated to 490-510°C in air at a rate of 1.5-2.5°C / min, and after being kept at this temperature for 1.7-2.1 hours, it is naturally cooled to room temperature to obtain 3D-MN Co3O4;
[0015] The mass molar ratio of N-CN to cobalt nitrate is 1g:1.13-1.26mol;
[0016] In the preparation step of the 3D-MN Co3O4, the drying temperature is 75-85°C and the drying time is 11.5-12.5 hours.
[0017] The preparation method of N-CN comprises dissolving glucose and sodium chloride in deionized water, freeze-drying the obtained mixed solution at -48 to -52°C for 23 to 25 hours, grinding and crushing the mixed solution and mixing it with urea to obtain a composite powder, and then heating the composite powder at 645 to 655°C in an Ar atmosphere for 1.5 to 2.6 hours, cooling the composite powder, washing it with water, and drying it to obtain N-CN;
[0018] The flow rate of the Ar atmosphere was 194-202 mL / min.
[0019] The mass ratio of the glucose, sodium chloride, deionized water and urea is 1:(17-22):(58-63):(0.9-1.2).
[0020] The GDC@3D-MN Co3O4 material prepared by the preparation method is used in preparing a solid oxide battery barrier layer.
[0021] Compared with the prior art, the present invention achieves the following beneficial effects:
[0022] The present invention proposes a preparation method of a composite heterostructure GDC@3D-MN Co3O4 material, in which GDC is compounded with a three-dimensional metal oxide nanomaterial, which is beneficial to better dispersion of GDC. NH4HCO3 is used as a precipitant, so that GDC can be better grown on the surface of 3D-MN Co3O4, and GDC is adjusted from grain boundary conduction to surface high ion conduction, which effectively improves the ion conductivity. The stability of the material can also be improved through covalent bond connection, avoiding the addition of subsequent sintering aids. When the barrier layer is prepared by high-temperature sintering, the crystal surface bonding degree can be improved, the sintering temperature can be reduced, the density of the barrier layer can be improved, the ion conductivity can be improved, and the ohmic impedance can be reduced.
[0023] When the GDC@3D-MN Co3O4 material of the present invention is used to prepare a battery barrier layer by high-temperature sintering, the sintering temperature can be reduced to 1200°C. The prepared battery barrier layer has a high density and an ohmic impedance of 1.27-2.12Ω•cm at 750°C. 2 , the ionic conductivity is 0.06-0.1 S / cm. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 TEM image of GDC@3D-MN Co3O4 powder prepared in Example 1;
[0025] Figure 2 is a SEM image of the composite material containing the barrier layer in Experimental Example 3;
[0026] in Figure 2 A is the SEM image of the composite material containing the GDC barrier layer. Figure 2 B is the SEM image of the composite material containing GDC@3D-MN Co3O4 barrier layer. DETAILED DESCRIPTION
[0027] Unless otherwise specified, all parts described in the present invention are parts by weight.
[0028] Example 1 Preparation method of a composite heterostructure GDC@3D-MN Co3O4 material
[0029] (1) Preparation of three-dimensional nitrogen-doped carbon network (N-CN)
[0030] 1 part of glucose and 20 parts of sodium chloride were dissolved in 60 parts of deionized water. The resulting mixed solution was freeze-dried at -50°C for 24 hours in a vacuum environment. After grinding, it was mixed with 1 part of urea to obtain a composite powder. The composite powder was then heated at 650°C in an Ar atmosphere (200 mL / min) for 2 hours. After cooling, the product was washed three times with deionized water and dried at 80°C overnight to obtain pure N-CN for later use.
[0031] (2) Preparation of 3D-MN Co3O4
[0032] 3D-MN Co3O4 was prepared by template method using three-dimensional nitrogen-doped carbon network (N-CN) as template.
[0033] The freshly prepared N-CN (0.033 g) was dispersed in a cobalt nitrate solution (20 mL; 2 mol / L), and after ultrasonic dispersion for 15 min, the resulting suspension was kept at 35 °C for 12 h. Then, the suspension was filtered, the filter cake was washed, and dried at 80 °C for 12 h. The resulting dry product was heated to 500 °C in air at a rate of 2 °C / min, kept at this temperature for 2 h, and naturally cooled to room temperature to obtain 3D-MN Co3O4.
[0034] (3) Preparation of GDC@3D-MN Co3O4 material
[0035] Press Ce 0.9 G 0.1 O 1.95 Ce(NO3)3·6H2O (analytical grade) and Gd(NO3)3·6H2O (analytical grade) were weighed in a stoichiometric ratio of 9:1. The two nitrates were dissolved in deionized water to obtain a nitrate solution with a total concentration of 0.1 mol / L.
[0036] 3D-MN Co3O4 was added to the nitrate solution, and after ultrasonic dispersion, it was placed in a 60°C water bath and stirred. Then, 0.1 mol / L NH4HCO3 solution was slowly added dropwise until the pH of the solution reached 7.5. The solution was allowed to stand to obtain a white precipitate. The precipitate was washed three times with deionized water and anhydrous ethanol by centrifugation, dried in an oven at 70°C for 24 h, and finally calcined at 750°C in an air atmosphere for 2 h to obtain GDC@3D-MN Co3O4 powder.
[0037] The mass ratio of the 3D-MN Co3O4 and Ce(NO3)3·6H2O is 1:2;
[0038] The molar ratio of the 3D-MN Co3O4 to NH4HCO3 is 1:9;
[0039] During the process of adding the NH4HCO3 solution dropwise and the process of standing, the temperature was maintained at 60°C.
[0040] Example 2 Preparation method of a composite heterostructure GDC@3D-MN Co3O4 material
[0041] (1) Preparation of three-dimensional nitrogen-doped carbon network (N-CN)
[0042] 1 part of glucose and 17 parts of sodium chloride were dissolved in 58 parts of deionized water. The resulting mixed solution was freeze-dried at -48°C in vacuum for 25 hours, ground and mixed with 0.9 parts of urea to obtain a composite powder. The composite powder was then heated at 645°C in an Ar atmosphere (194 mL / min) for 2.6 hours. After cooling, the product was washed three times with deionized water and dried at 77°C overnight to obtain pure N-CN for later use.
[0043] (2) Preparation of 3D-MN Co3O4
[0044] 3D-MN Co3O4 was prepared by template method using three-dimensional nitrogen-doped carbon network (N-CN) as template.
[0045] The freshly prepared N-CN (0.03 g) was dispersed in a cobalt nitrate solution (17 mL; 2 mol / L), and after ultrasonic dispersion for 12 min, the resulting suspension was kept at 33 °C for 13 h. Then, the suspension was filtered, the filter cake was washed, and dried at 75 °C for 12.5 h. The resulting dry product was heated to 490 °C in air at a rate of 1.5 °C / min, kept at this temperature for 2.1 h, and naturally cooled to room temperature to obtain 3D-MN Co3O4.
[0046] (3) Preparation of GDC@3D-MN Co3O4 material
[0047] Press Ce 0.9 G 0.1 O 1.95 Ce(NO3)3·6H2O (analytical grade) and Gd(NO3)3·6H2O (analytical grade) were weighed in a stoichiometric ratio. The molar ratio of Ce(NO3)3·6H2O to Gd(NO3)3·6H2O was 8.8:1. The two nitrates were dissolved in deionized water to obtain a nitrate solution with a total concentration of 0.08 mol / L.
[0048] 3D-MN Co3O4 was added to the nitrate solution, and after ultrasonic dispersion, it was placed in a 57°C water bath and stirred. Then, 0.1 mol / L NH4HCO3 solution was slowly added dropwise until the pH of the solution reached 7.7. The solution was allowed to stand to obtain a white precipitate. The precipitate was washed three times with deionized water and anhydrous ethanol by centrifugation, dried in an oven at 68°C for 24.5 h, and finally calcined at 745°C in an air atmosphere for 2.3 h to obtain GDC@3D-MN Co3O4 powder.
[0049] The mass ratio of the 3D-MN Co3O4 and Ce(NO3)3·6H2O is 1:1;
[0050] The molar ratio of the 3D-MN Co3O4 to NH4HCO3 is 1:8.7;
[0051] During the process of adding the NH4HCO3 solution dropwise and the process of standing, the temperature was maintained at 57°C.
[0052] Example 3 Preparation method of a composite heterostructure GDC@3D-MN Co3O4 material
[0053] (1) Preparation of three-dimensional nitrogen-doped carbon network (N-CN)
[0054] 1 part of glucose and 22 parts of sodium chloride were dissolved in 63 parts of deionized water. The resulting mixed solution was freeze-dried at -52°C in vacuum for 23 hours, ground and mixed with 1.2 parts of urea to obtain a composite powder. The composite powder was then heated at 655°C in an Ar atmosphere (202 mL / min) for 1.5 hours. After cooling, the product was washed three times with deionized water and dried at 85°C overnight to obtain pure N-CN for later use.
[0055] (2) Preparation of 3D-MN Co3O4
[0056] 3D-MN Co3O4 was prepared by template method using three-dimensional nitrogen-doped carbon network (N-CN) as template.
[0057] The freshly prepared N-CN (0.035 g) was dispersed in a cobalt nitrate solution (22 mL; 2 mol / L), and after ultrasonic dispersion for 17 min, the resulting suspension was kept at 38 °C for 11 h. Then, the suspension was filtered, the filter cake was washed, and dried at 85 °C for 11.5 h. The resulting dry product was heated to 510 °C in air at a rate of 2.5 °C / min, kept at this temperature for 1.7 h, and naturally cooled to room temperature to obtain 3D-MN Co3O4.
[0058] (3) Preparation of GDC@3D-MN Co3O4 material
[0059] Press Ce 0.9 G0.1 O 1.95 Ce(NO3)3·6H2O (analytical grade) and Gd(NO3)3·6H2O (analytical grade) were weighed in a stoichiometric ratio. The molar ratio of Ce(NO3)3·6H2O to Gd(NO3)3·6H2O was 9.2:1. The two nitrates were dissolved in deionized water to obtain a nitrate solution with a total concentration of 0.13 mol / L.
[0060] 3D-MN Co3O4 was added to the nitrate solution, and after ultrasonic dispersion, it was placed in a 63°C water bath and stirred. Then, 0.1 mol / L NH4HCO3 solution was slowly added dropwise until the pH of the solution reached 8.0. The solution was allowed to stand to obtain a white precipitate. The precipitate was washed three times by centrifugation with deionized water and anhydrous ethanol respectively, and then dried in an oven at 73°C for 23.5 h. Finally, it was calcined at 755°C in an air atmosphere for 1.7 h to obtain GDC@3D-MN Co3O4 powder.
[0061] The mass ratio of the 3D-MN Co3O4 and Ce(NO3)3·6H2O is 1:4;
[0062] The molar ratio of the 3D-MN Co3O4 to NH4HCO3 is 1: 9.3;
[0063] During the process of adding the NH4HCO3 solution dropwise and the process of standing, the temperature was maintained at 63°C.
[0064] Comparative Example 1 Preparation of GDC Material
[0065] Based on Example 1, the changes are as follows: Step (1) and Step (2) are omitted, and 3D-MNCo3O4 is not added in Step (3).
[0066] The specific preparation method is as follows:
[0067] Press Ce 0.9 G 0.1 O 1.95 Ce(NO3)3·6H2O (analytical grade) and Gd(NO3)3·6H2O (analytical grade) were weighed in a stoichiometric ratio of 9:1. The two nitrates were dissolved in deionized water to obtain a nitrate solution with a total concentration of 0.1 mol / L.
[0068] The nitrate solution was placed in a 60°C water bath and stirred. Then, 0.1 mol / L NH4HCO3 solution was slowly added dropwise to the nitrate solution until the pH of the solution reached 7.5. The solution was allowed to stand to obtain a white precipitate. The precipitate was washed three times by centrifugation with deionized water and anhydrous ethanol respectively. The precipitate was dried in an oven at 70°C for 24 hours. Finally, the precipitate was calcined at 750°C for 2 hours in an air atmosphere to obtain GDC powder.
[0069] During the process of adding the NH4HCO3 solution dropwise and the process of standing, the temperature was maintained at 60°C.
[0070] Test Example 1
[0071] The GDC@3D-MN Co3O4 powder prepared in Examples 1-3 and the GDC powder prepared in Comparative Example 1 were pressed into green round tablets with a diameter of 10 mm and a thickness of 1 mm using a tablet pressing mold at a pressure of 260 MPa on a uniaxial press. The pressure was maintained for 3 minutes and then sintered at 1200°C for 2 hours to obtain a battery barrier layer.
[0072] Evenly apply conductive glue and silver paste on both sides of the battery barrier layer, connect two silver wires, detect the ohmic impedance at 750℃, and calculate the ionic conductivity. The calculation formula of ionic conductivity is as follows:
[0073]
[0074] l is the thickness of the battery barrier layer, R is the ohmic resistance, and S is the effective area.
[0075] The test results are shown in Table 1.
[0076] Table 1 Test results of ohmic impedance and ionic conductivity
[0077]
[0078] It can be seen that the battery barrier layer prepared by using GDC@3D-MN Co3O4 powder has significantly lower ohmic impedance and significantly improved ionic conductivity compared with the battery barrier layer prepared by using GDC powder.
[0079] Test Example 2
[0080] The GDC@3D-MN Co3O4 powder prepared in Example 1 was observed under a transmission electron microscope (TEM). Figure 1 .
[0081] Depend on Figure 1 It can be seen that the present invention has successfully synthesized GDC, and GDC is evenly distributed on the three-dimensional 3D-MN Co3O4 to form a three-dimensional encapsulation structure.
[0082] Test Example 3
[0083] The GDC@3D-MN Co3O4 powder prepared in Example 1 was pressed into a green blank with a diameter of 10 mm and a thickness of 1 mm by a tablet pressing mold on a uniaxial press at a pressure of 260 MPa for 3 minutes, and then sintered at 1200°C for 2 hours to obtain a GDC@3D-MN Co3O4 barrier layer. The GDC@3D-MN Co3O4 barrier layer was then screen-printed on the surface of the YSZ by screen printing. After sintering at 1200°C for 2 hours, a cathode layer LSCF was screen-printed on the surface of the GDC@3D-MN Co3O4 barrier layer. After sintering at 1050°C for 2 hours, the obtained composite material was observed under a scanning electron microscope (SEM). The SEM image is shown in FIG. Figure 2 B.
[0084] The GDC powder prepared in Comparative Example 1 was pressed into a green blank with a diameter of 10 mm and a thickness of 1 mm by a tablet pressing mold on a uniaxial press at a pressure of 260 MPa for 3 minutes, and then sintered at 1200° C. for 2 hours to obtain a GDC barrier layer. The GDC barrier layer was then screen-printed on the surface of the YSZ by screen printing. After sintering at 1200° C. for 2 hours, a cathode layer LSCF was screen-printed on the surface of the GDC barrier layer. After sintering at 1050° C. for 2 hours, the obtained composite material was observed under a scanning electron microscope (SEM). The SEM image is shown in FIG. Figure 2 A.
[0085] Depend on Figure 2 It can be seen that the GDC@3D-MN Co3O4 barrier layer has a denser structure than the GDC barrier layer, can play a better barrier role, and has better bonding performance with the YSZ layer.
Claims
1. A method for preparing a composite heterostructure GDC@3D-MN Co3O4 material, characterized by: The preparation method comprises the following steps: dissolving Ce(NO3)3·6H2O and Gd(NO3)3·6H2O in deionized water to obtain a nitrate solution, adding 3D-MN Co3O4 to the nitrate solution, uniformly dispersing the solution, heating the solution to 57-63°C, slowly adding NH4HCO3 solution dropwise under stirring until the pH value of the solution reaches 7.5-8.0, and allowing the solution to stand to obtain a white precipitate. The GDC@3D-MN Co3O4 powder material is obtained through washing, drying, and calcining.
2. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 1, characterized in that: The molar ratio of Ce(NO3)3·6H2O and Gd(NO3)3·6H2O is 8.8-9.2:1; the mass ratio of 3D-MN Co3O4 and Ce(NO3)3·6H2O is 1:1-4.
3. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 1, characterized in that: The concentration of the nitrate solution is 0.08-0.13 mol / L; the molar ratio of the 3D-MN Co3O4 to NH4HCO3 is 1:8.7-9.
3.
4. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 1, characterized in that: The temperature was controlled at 57-63° C. during the dropwise addition of the NH 4 HCO 3 solution and the standing process.
5. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 1, characterized in that: The calcination temperature is 745-755° C., and the calcination time is 1.7-2.3 hours.
6. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 1, characterized in that: The preparation method of the 3D-MN Co3O4 comprises dispersing N-CN in a cobalt nitrate solution, maintaining the resulting suspension at 33-38°C for 11-13 hours after uniform dispersion; filtering the suspension, washing the filter cake, and drying the resulting dry product in air at a rate of 1.5-2.5°C / min to 490-510°C, maintaining the dried product at this temperature for 1.7-2.1 hours, and then naturally cooling it to room temperature to obtain 3D-MN Co3O4.
7. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 6, characterized in that: The mass molar ratio of the N—CN to cobalt nitrate is 1 g:1.13-1.26 mol.
8. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 6 or 7, characterized in that: The preparation method of N-CN comprises the following steps: dissolving glucose and sodium chloride in deionized water, freeze-drying the obtained mixed solution at -48 to -52°C in a vacuum environment for 23 to 25 hours, grinding and pulverizing the mixed solution and mixing it with urea to obtain a composite powder, and then heating the composite powder at 645 to 655°C in an Ar atmosphere for 1.5 to 2.6 hours, cooling, washing, and drying the resulting N-CN.
9. The method for preparing a composite heterostructure GDC@3D-MN Co3O4 material according to claim 8, characterized in that: The mass ratio of the glucose, sodium chloride, deionized water and urea is 1:(17-22):(58-63):(0.9-1.2).
10. Use of the GDC@3D-MN Co3O4 material prepared by the preparation method of claim 1 in preparing a barrier layer for a solid oxide battery.