Blue high-brightness high-strength pervious concrete and preparation method thereof

By using blue glass coarse aggregate and fine aggregate combined with ordinary silicon cement and other materials, the problem of insufficient mechanical properties of permeable concrete is solved, the preparation of high-brightness and high-strength permeable concrete is achieved, the preparation process is simplified and energy consumption is reduced, improving Improves nighttime brightness and safety.

CN118724534APending Publication Date: 2024-10-01安徽建工集团建材科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410894708.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for existing permeable concrete to ensure high mechanical properties while ensuring water permeability, and the preparation process is complex and energy-consuming. There is a need for research on high-strength permeable concrete materials.

Method used

Blue glass coarse aggregate and fine aggregate are used in combination with silicon cement, mineral powder, gravel and nano-glass powder. The mechanical properties of the concrete are improved through grinding and grinding, and the mechanical properties of the concrete are improved through the use of nano-glass powder, cellulose ether and sodium carbonate. The reinforcing agent is prepared by mixing, heating and stirring to modify the rheological properties and early activity of cement slurry.

Benefits of technology

Green, low-carbon, simple to prepare, high-brightness and high-strength permeable concrete has been realized, which improves the mechanical properties and anti-skid properties. At the same time, the reflection effect of blue glass improves the brightness at night and reduces the probability of night accidents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004928580350000071
    Figure BDA0004928580350000071
Patent Text Reader

Abstract

The invention is suitable for the technical field of concrete, and provides blue high-brightness high-strength pervious concrete, which is prepared from the following raw materials in parts by weight: 280 to 320 parts of ordinary portland cement, 50 to 100 parts of mineral powder, 300 to 500 parts of blue glass coarse aggregate, 800 to 1000 parts of gravel, 50 to 100 parts of blue glass fine aggregate, 130 to 150 parts of water, 4.5 to 5.5 parts of polycarboxylic acid water reducing agent and 0.2 to 0.5 part of reinforcing agent. The invention also provides a preparation method of the blue high-brightness high-strength pervious concrete. Waste blue glass is subjected to galling treatment, so that the connecting area and contact sites of cement paste and the blue glass coarse aggregate are increased, the mechanical property of the pervious concrete is improved, the surface friction coefficient of the blue glass coarse aggregate subjected to galling treatment is also increased, and the skid resistance of the pervious concrete is improved; the blue glass coarse and fine aggregates and the nano glass powder can reflect light to form a high-brightness road surface under the action of night light due to the special crystal structure, and are green, low-carbon, simple to prepare, high in brightness and high in strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete, and in particular relates to a blue high-brightness high-strength permeable concrete and a preparation method thereof. Background Art

[0002] Permeable concrete is a new type of concrete material with excellent water permeability, good environmental performance and heat dissipation performance. It can effectively alleviate the local waterlogging and waterlogging problems in cities. In combination with the urban rainwater recycling system, it can realize the secondary reuse of natural water resources. Therefore, permeable concrete is increasingly used in garden landscapes. However, at present, permeable concrete has good water permeability, but it is difficult to ensure high mechanical properties and is prone to early damage. Therefore, it is urgent to study high-strength permeable concrete materials while ensuring permeability.

[0003] The presence of high-brightness pavement can create a warm and comfortable environment at dusk and night, making the city more vibrant. At the same time, it not only provides brightness, but also plays an important role in improving urban safety, beautifying the city's night scene and promoting social activities.

[0004] The patent application with publication number CN115626799A discloses a colored permeable concrete and a preparation method thereof, wherein the colored permeable concrete comprises the following raw materials in parts by weight: 0-2% admixture, 85-105 parts of water, 340-375 parts of cement, 20-40 parts of color powder, 35-50 parts of admixture, 1200-1300 parts of coarse aggregate, 1-3 parts of polyimide fiber, 0.8-2 parts of polytetrafluoroethylene fiber, and 2-5 parts of silicone emulsion; the preparation process comprises the following steps: dry-mixing the coarse aggregate and cement until uniform; continuing to add water, admixture, admixture, polyimide fiber, and polytetrafluoroethylene fiber and stirring and mixing until uniform; continuing to add color powder and silicone emulsion and stirring until uniform; and obtaining the finished product. The above technical scheme has the advantage of improving the color stability of the colored permeable concrete, and the colored permeable concrete is obtained by molding, but additional color powder needs to be added to supplement the color, which consumes a lot of energy and is complicated to prepare.

[0005] The patent application with publication number CN116177931A discloses a high-strength permeable concrete and a preparation method thereof. The high-strength permeable concrete includes raw materials, a hardener and a curing agent. The raw materials include the following components by weight: 70-85 parts of water, 300-400 parts of cement, 60-110 parts of mineral powder, 50-70 parts of fly ash and 80-100 parts of hard ceramic particles; the hardener includes the following components by weight: 20-30 parts of early strength agent, 30-40 parts of aluminum sulfate, 20-35 parts of silicon dioxide, and 20-40 parts of water-soluble fluoride resin. The permeable concrete of the above technical solution has excellent mechanical properties, but has problems such as more components, complex preparation, and high energy consumption.

[0006] The patent application with publication number CN117865567A discloses an environmentally friendly high-strength permeable concrete and its preparation method. First, (S)-2-amino-3-hydroxy-3-methylbutyric acid hydrochloride, thionyl chloride, 2-pyrazol-1-ylethane hydrazine, and cinnamaldehyde are used to react to generate Schiff base compounds. The amide pyrazolyl and Schiff base coexist to prevent the concrete from decreasing porosity due to mold, moss, etc. Then, cross-linking forms an antibacterial hydrogel and wraps it on the surface of the carbon nanotube hollow fiber, so that the fibers and the fibers, and the fibers and the concrete are cross-linked with each other, forming a hard three-dimensional mesh fiber protective film on the surface of the concrete and the inner wall of the pores, which is conducive to maintaining the water permeability and strength of the concrete. At the same time, a layer of calcium ions is also adsorbed on the surface of the hydrogel, which can form sediments when encountering rainwater and coat the surface of the concrete to further enhance the water permeability and strength. The above technical scheme improves the mechanical properties of permeable concrete through physical and chemical synergy, but the preparation method has about ten chemicals such as 2-pyrazol-1-ylethane hydrazine and is extremely complicated to prepare.

[0007] In summary, the existing technical solutions have the problems of complex preparation of high-strength permeable concrete, complex chemical composition, high energy consumption, etc. Summary of the invention

[0008] The purpose of the embodiments of the present invention is to provide a blue high-brightness high-strength permeable concrete, aiming to solve the problems raised in the above-mentioned background technology.

[0009] The embodiment of the present invention is implemented as follows: a blue high-brightness high-strength permeable concrete includes the following raw materials in parts by weight: 280-320 parts of ordinary silica cement, 50-100 parts of mineral powder, 300-500 parts of blue glass coarse aggregate, 800-1000 parts of crushed stone, 50-100 parts of blue glass fine aggregate, 130-150 parts of water, 4.5-5.5 parts of polycarboxylic acid water reducer, and 0.2-0.5 parts of reinforcing agent.

[0010] Preferably, the size of the blue glass coarse aggregate is 4-8 mm.

[0011] Preferably, the fineness modulus of the blue glass fine aggregate is 0.1 to 0.3.

[0012] Preferably, the grade of ordinary silica cement is 42.5.

[0013] Another object of the embodiment of the present invention is to provide a method for preparing blue high-brightness high-strength permeable concrete, comprising the following steps:

[0014] (1) Grinding and roughening the discarded blue glass, crushing and screening the roughened blue glass coarse aggregate of 4 to 8 mm;

[0015] (2) crushing or grinding the remaining waste blue glass to prepare blue glass fine aggregate with a fineness modulus of 0.1 to 0.3;

[0016] (3) preparing a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 7-9: 0.5-1: 0.01-0.02: 20-30;

[0017] (4) Weigh the following ingredients in parts by weight: 280-320 parts of ordinary silica cement, 50-100 parts of mineral powder, 300-500 parts of blue glass coarse aggregate, 800-1000 parts of crushed stone, 50-100 parts of blue glass fine aggregate, 130-150 parts of water, 4.5-5.5 parts of polycarboxylic acid water reducer, and 0.2-0.5 parts of reinforcing agent, and mix well.

[0018] Preferably, in step (2), the grinding ball-to-material ratio is 7-9:1-3, and the rotation speed is 600-650 r / min.

[0019] Preferably, in step (3), the temperature of the constant temperature water bath is 40-50° C., and the stirring frequency is 100-150 Hz.

[0020] The blue high-brightness high-strength permeable concrete provided by the embodiment of the present invention is green and low-carbon, easy to prepare, high-brightness and high-strength. The contact area and contact points between cement slurry and blue glass coarse aggregate are increased by roughening the waste blue glass, thereby improving the mechanical properties of the permeable concrete. The roughened blue glass coarse aggregate also increases the surface friction coefficient, thereby improving the anti-slip property of the permeable concrete.

[0021] Blue glass coarse and fine aggregates and nano glass powder can reflect light at night to form a bright road surface due to their special crystal structure;

[0022] Blue glass fine aggregate is mixed with cementitious materials to form cement mortar, which can improve the bonding surface and bonding sites between aggregate and paste, and further improve the mechanical properties of permeable concrete;

[0023] Nano glass powder, cellulose ether, sodium carbonate and water are mixed, heated and stirred. Sodium carbonate can be used as a dispersant to improve the dispersibility of nano glass powder in the solution. Cellulose ether and nano glass powder can modify the rheological properties of cement slurry through chemical and physical methods. In addition, nano glass powder can improve the early activity of cement slurry through the nucleation effect. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] A blue high-brightness high-strength permeable concrete, the preparation method of which comprises the following steps:

[0026] (1) Grind and roughen the discarded blue glass with a hand-held grinder, and then put it into a crusher to crush and screen the blue glass coarse aggregate of 4 to 8 mm;

[0027] (2) crushing or grinding the remaining waste blue glass to prepare blue glass fine aggregate with a fineness modulus of 0.1 to 0.3, with a grinding ratio of 7 to 9:1 to 3 and a rotation speed of 600 to 650 r / min;

[0028] (3) preparing a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 7-9: 0.5-1: 0.01-0.02: 20-30, wherein the temperature of the constant temperature water bath is 40-50° C. and the stirring frequency is 100-150 Hz;

[0029] (4) Weigh the following parts by weight: 280-320 parts of ordinary silica cement (grade 42.5), 50-100 parts of mineral powder, 300-500 parts of blue glass coarse aggregate, 800-1000 parts of crushed stone, 50-100 parts of blue glass fine aggregate, 130-150 parts of water, 4.5-5.5 parts of polycarboxylic acid water reducer, and 0.2-0.5 parts of reinforcing agent, and mix well.

[0030] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0031] Example 1

[0032] A blue high-brightness high-strength permeable concrete, the preparation method of which comprises the following steps:

[0033] (1) Grind and roughen the discarded blue glass with a hand-held grinder, and then put it into a crusher to crush and screen the blue glass coarse aggregate of 4 to 8 mm;

[0034] (2) The remaining waste blue glass is further crushed or ground to produce blue glass fine aggregate with a fineness modulus of 0.2;

[0035] (3) Prepare a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 8:1:0.01:25.

[0036] (4) Weigh the following ingredients according to their weight: 300 kg of ordinary silica cement, 100 kg of mineral powder, 400 kg of blue glass coarse aggregate, 900 kg of crushed stone, 50 kg of blue glass fine aggregate, 145 kg of water, 5.5 kg of polycarboxylic acid water reducer, and 0.2 kg of reinforcing agent, and mix well.

[0037] Example 2

[0038] A blue high-brightness high-strength permeable concrete, the preparation method of which comprises the following steps:

[0039] (1) Grind and roughen the discarded blue glass with a hand-held grinder, and then put it into a crusher to crush and screen the blue glass coarse aggregate of 4 to 8 mm;

[0040] (2) The remaining waste blue glass is further crushed or ground to produce blue glass fine aggregate with a fineness modulus of 0.2;

[0041] (3) Prepare a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 8:1:0.01:25.

[0042] (4) Weigh the following parts by weight: 300 kg of ordinary silica cement, 100 kg of mineral powder, 450 kg of blue glass coarse aggregate, 850 kg of crushed stone, 50 kg of blue glass fine aggregate, 145 kg of water, 5.5 kg of polycarboxylic acid water reducer, and 0.2 kg of reinforcing agent, and mix well.

[0043] Example 3

[0044] A blue high-brightness high-strength permeable concrete, the preparation method of which comprises the following steps:

[0045] (1) Grind and roughen the discarded blue glass with a hand-held grinder, and then put it into a crusher to crush and screen the blue glass coarse aggregate of 4 to 8 mm;

[0046] (2) The remaining waste blue glass is further crushed or ground to produce blue glass fine aggregate with a fineness modulus of 0.2;

[0047] (3) Prepare a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 8:1:0.01:25.

[0048] (4) Weigh the following ingredients according to their weight: 300 kg of ordinary silica cement, 100 kg of mineral powder, 500 kg of blue glass coarse aggregate, 800 kg of crushed stone, 50 kg of blue glass fine aggregate, 145 kg of water, 5.5 kg of polycarboxylic acid water reducer, and 0.2 kg of reinforcing agent, and mix well.

[0049] Comparative Example 1

[0050] A concrete preparation method comprises the following steps:

[0051] (1) Prepare a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 8:1:0.01:25.

[0052] (2) Weigh the following ingredients according to their weight: 300 kg of ordinary silica cement, 100 kg of mineral powder, 1,300 kg of crushed stone, 50 kg of fine aggregate, 145 kg of water, 5.5 kg of polycarboxylate water reducer, and 0.2 kg of reinforcing agent, and mix well.

[0053] Performance Testing:

[0054] The surface appearance, mechanical properties and reflective properties of Examples 1-3 and Comparative Example 1 were measured, as shown in Table 1:

[0055] Table 1

[0056]

[0057]

[0058] It can be seen from Table 1 that: relative to comparative example 1, the surface appearance of the concrete prepared in the embodiment of the present invention presents blue spots, and the color of the concrete is no longer monotonous; the 3d compressive strength is increased by 3.1-5.1 MPa relative to the control group, the early mechanical properties are improved, the 28d compressive strength is increased by 3-5.5 MPa, and the later mechanical properties increase steadily; after adding waste blue glass coarse and fine aggregates, the reflection effect at night is significantly enhanced, which is beneficial to improve the brightness of the road surface at night and reduce the probability of accidents at night.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A blue high-brightness high-strength permeable concrete, characterized in that: The method comprises the following raw materials in parts by weight: 280-320 parts of ordinary silica cement, 50-100 parts of mineral powder, 300-500 parts of blue glass coarse aggregate, 800-1000 parts of crushed stone, 50-100 parts of blue glass fine aggregate, 130-150 parts of water, 4.5-5.5 parts of polycarboxylic acid water reducer, and 0.2-0.5 parts of reinforcing agent.

2. The blue high-brightness high-strength permeable concrete according to claim 1 is characterized in that: The size of the blue glass coarse aggregate is 4-8 mm.

3. The blue high-brightness high-strength permeable concrete according to claim 1 is characterized in that: The fineness modulus of the blue glass fine aggregate is 0.1-0.

3.

4. The blue high-brightness high-strength permeable concrete according to claim 1 is characterized in that: The grade of the ordinary silica cement is 42.

5.

5. A method for preparing blue high-brightness high-strength permeable concrete as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Grind and roughen the discarded blue glass, crush and screen the roughened blue glass coarse aggregates of 4-8 mm; (2) The remaining waste blue glass is further crushed or ground to prepare blue glass fine aggregate with a fineness modulus of 0.1 to 0.3; (3) Prepare a reinforcing agent by stirring nano glass powder, cellulose ether, sodium carbonate and water in a constant temperature water bath at a ratio of 7-9: 0.5-1: 0.01-0.02: 20-30; (4) Weigh the following ingredients in parts by weight: 280-320 parts of ordinary silica cement, 50-100 parts of mineral powder, 300-500 parts of blue glass coarse aggregate, 800-1000 parts of crushed stone, 50-100 parts of blue glass fine aggregate, 130-150 parts of water, 4.5-5.5 parts of polycarboxylic acid water reducer, and 0.2-0.5 parts of reinforcing agent, and mix well.

6. The method for preparing blue high-brightness high-strength permeable concrete according to claim 5, characterized in that: In step (2), the grinding ball-to-material ratio is 7-9:1-3, and the rotation speed is 600-650 r / min.

7. The method for preparing blue high-brightness high-strength permeable concrete according to claim 5, characterized in that: In step (3), the temperature of the constant temperature water bath is 40-50° C., and the stirring frequency is 100-150 Hz.

Citation Information

Patent Citations

  • External wall heat-insulation material for constructional engineering and preparation method thereof

    CN109704806A

  • Cement-based capillary crystalline waterproof material based on nanosilicon-based material and preparation method and application thereof

    CN110105025A

  • Concrete prepared from waste glass and preparation method thereof

    CN114907074A

  • Cement admixture and cement composition

    JP1992164845A

  • Semiconductor devices

    KR1020250108872A